CN104562085A - 一种粗铅的电解精炼方法 - Google Patents

一种粗铅的电解精炼方法 Download PDF

Info

Publication number
CN104562085A
CN104562085A CN201410800014.1A CN201410800014A CN104562085A CN 104562085 A CN104562085 A CN 104562085A CN 201410800014 A CN201410800014 A CN 201410800014A CN 104562085 A CN104562085 A CN 104562085A
Authority
CN
China
Prior art keywords
lead
electrolytic solution
processed
bullion
electrolytic
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410800014.1A
Other languages
English (en)
Inventor
李大志
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WUHU JINLONG MOLD FORGING CO Ltd
Original Assignee
WUHU JINLONG MOLD FORGING CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUHU JINLONG MOLD FORGING CO Ltd filed Critical WUHU JINLONG MOLD FORGING CO Ltd
Priority to CN201410800014.1A priority Critical patent/CN104562085A/zh
Publication of CN104562085A publication Critical patent/CN104562085A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种粗铅的电解精炼方法,属于有色金属领域。其包括以下步骤:(1)电极的制备;(2)电解溶液的准备;(3)电解;(4)加入添加剂;(5)后期处理。本发明解决了现有粗铅冶炼的过程中,因存在杂质造成铅纯度降低以及重金属浪费的问题,具有方法简单,成本低,加工容易的优点。

Description

一种粗铅的电解精炼方法
技术领域
本发明属于有色金属领域,更具体地说,涉及一种用于粗铅精炼的方法。
背景技术
铅在目前工业上应用广泛,尤其是在电气工业部门用量最多,主要用来制造蓄电池、各种电缆保护皮、熔断保险丝等。 铅板和铅管常作冶炼和化工设备防腐的耐酸衬里、防腐盖,铅还用做原子能工业和X光的防护层及防护屏。铅的化合物用于颜料工业、玻璃工业、石油工业及医药部门等。但铅在加工提炼的过程中,除了含有Cu、Sn、As、Sb等杂质外,还含有贵金属以及其他杂质。由于杂质的存在,不仅使得铅的硬度增加,延性和抗蚀性降低,不适合工业使用,而且对于其中的贵金属也造成了浪费。
发明内容
针对现有粗铅冶炼的过程中,因存在杂质造成铅纯度降低以及重金属浪费的问题,本发明提供一种粗铅的电解精炼方法,通过电解的方法来精炼铅,使铅的纯度得到了提高,也实现了贵金属的回收利用。
为解决上述问题,本发明采用如下的技术方案。
一种粗铅的电解精炼方法,包括以下步骤:
(1)电极的制备:
利用纯铅加工成始极片,作为阴极,将粗铅锭加工成薄片,作为阳极;
(2)电解溶液的准备:
将硅氟酸铅和游离硅氟酸按照一定的比例制成电解溶液;
(3)电解:
将阴极和阳极按照一定间距装入含有电解溶液的电解槽中,并在两端接入直流电,电流密度为170-190A/m2
(4)加入添加剂:
将动物硅胶或者木质磺酸钠加入到电解液中;
(5)后期处理:
利用分离装置对阴极上精炼得到的铅进行分离,并对阳极泥进一步处理,回收贵金属。
优选的,所述的步骤(3)中,电流密度为180A/m2
相比于现有技术,本发明的有益效果为:
(1)本发明利用电解的方法来实现铅的精炼,不仅使铅的纯度得到了提高,也实现了贵金属的回收利用。
(2)本发明方法简单,成本低,加工容易。
具体实施方式
下面结合实施例对本发明进行详细描述。
实施例1
一种粗铅的电解精炼方法,包括以下步骤:
(1)电极的制备:
利用纯铅加工成始极片,作为阴极,将粗铅锭加工成薄片,作为阳极;
(2)电解溶液的准备:
将硅氟酸铅和游离硅氟酸按照一定的比例制成电解溶液;
(3)电解:
将阴极和阳极按照一定间距装入含有电解溶液的电解槽中,并在两端接入直流电,电流密度为180A/m2
(4)加入添加剂:
将动物硅胶或者木质磺酸钠加入到电解液中;
(5)后期处理:
利用分离装置对阴极上精炼得到的铅进行分离,并对阳极泥进一步处理,回收贵金属。

Claims (2)

1.一种粗铅的电解精炼方法,其特征在于以下步骤:
(1)电极的制备:
利用纯铅加工成始极片,作为阴极,将粗铅锭加工成薄片,作为阳极;
(2)电解溶液的准备:
将硅氟酸铅和游离硅氟酸按照一定的比例制成电解溶液;
(3)电解:
将阴极和阳极按照一定间距装入含有电解溶液的电解槽中,并在两端接入直流电,电流密度为170-190A/m2
(4)加入添加剂:
将动物硅胶或者木质磺酸钠加入到电解液中;
(5)后期处理:
利用分离装置对阴极上精炼得到的铅进行分离,并对阳极泥进一步处理,回收贵金属。
2.根据权利要求1所述的一种粗铅的电解精炼方法,其特征在于,所述的步骤(3)中,电流密度为180A/m2
CN201410800014.1A 2014-12-22 2014-12-22 一种粗铅的电解精炼方法 Pending CN104562085A (zh)