CN104088173B - 一种涤棉织物靛蓝染料同色染色的方法 - Google Patents

一种涤棉织物靛蓝染料同色染色的方法 Download PDF

Info

Publication number
CN104088173B
CN104088173B CN201410256555.2A CN201410256555A CN104088173B CN 104088173 B CN104088173 B CN 104088173B CN 201410256555 A CN201410256555 A CN 201410256555A CN 104088173 B CN104088173 B CN 104088173B
Authority
CN
China
Prior art keywords
dye
polyester
cotton fabric
bath
bipseudoindoxyl
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201410256555.2A
Other languages
English (en)
Other versions
CN104088173A (zh
Inventor
曹机良
孟春丽
王延伟
魏媛
许志忠
程献伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Henan Institute of Engineering
Original Assignee
Henan Institute of Engineering
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Henan Institute of Engineering filed Critical Henan Institute of Engineering
Priority to CN201410256555.2A priority Critical patent/CN104088173B/zh
Publication of CN104088173A publication Critical patent/CN104088173A/zh
Application granted granted Critical
Publication of CN104088173B publication Critical patent/CN104088173B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,在染浴中加入靛蓝染料、保险粉和氢氧化钠,升温至40~80℃,保温10~50min使靛蓝染料还原,然后加入载体和氯化钠,将涤棉织物投入染浴中,升温至80~100℃,保温20~90min;在另一个染浴中加入靛蓝染料、保险粉和氢氧化钠,升温至40~80℃,保温10~50min使靛蓝染料还原,将染色后的涤棉织物投入该染浴中,升温至20~60℃,保温30~60min;最后将染色织物水洗、皂洗、水洗、烘干或晾干。本发明采用两浴两步染色法对涤棉织物进行染色,使涤纶和棉织物有较好的同色性且达到满意的染色深度,工艺简单可行。

Description

一种涤棉织物靛蓝染料同色染色的方法
技术领域
本发明属于染整技术领域,涉及一种采用靛蓝染料对涤棉混纺或交织物进行染色的方法,尤其能实现涤棉靛蓝染色织物有较好的同色性和较高的染色深度。
背景技术
牛仔服起源于美国,起初牛仔服是为了解决裤子不结实的问题而出现,但随着牛仔服的发展,其作为一种时尚流行深受人们的青睐。随着人们生活质量提高,对服饰的要求也不断提高,要求牛仔服向着多样化、个性化、功能化等方面发展。涤纶织物有优良的保形性和抗皱性,且有优异的“洗可穿”性,以涤纶为原料制成的牛涤棉仔裤挺阔不皱,经久耐用,外形美观。棉涤牛仔服具有光泽好,色彩艳,亮度高等特点,突破了传统牛仔布布面沉闷、颜色单一的风格,为整个牛仔家族注入新活力。当前牛仔面料的多采用靛蓝染料染色,但染色时存在涤棉混纺或交织物很难染得同色,且染色深度不高的问题。发明专利CN1958899A公开了一种靛蓝牛仔灯芯绒的生产工艺,可制备涤棉织物作为牛仔面料,该工艺中涤纶作为原色纱线未经靛蓝染料染色;文献[染料与染色,2009,46 (1) ]对靛蓝染料涤棉织物染色进行探究,但其未对涤纶和棉织物同色性进行探讨,且染色温度为120℃,此染色适合涤纶的染色,棉织物上染较少。
发明内容
本发明所要解决的技术问题是针对当前涤棉混纺或交织物染色时,棉织物需在低温条件下染色而涤纶需在高温条件下才能上色,两种组分很难染得同色,且当前纯棉牛仔面料布面沉闷、颜色单一,保形性、抗皱性差,牢度差,不耐用的问题,提供一种两浴两步法对涤棉进行染色,使涤纶和棉织物获得良好的同色性且具有满意的染色深度,染色织物的皂洗和摩擦牢度相对于纯棉牛仔面料有很大的提高。
为解决上述技术问题,本发明采用以下技术方案:一种涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料0.05~8%owf,保险粉2~50g/L,氢氧化钠0.5~8g/L,以0.5~2℃/min的升温速度升温至40~80℃,保温10~50min使靛蓝染料还原,然后加入载体和氯化钠,将涤棉织物按浴比1:10~100投入染浴中,以0.5~3℃/min的升温速度升温至80~100℃,保温20~90min;
(2)在另一个染浴中加入靛蓝染料0.5~6%owf,保险粉3~40g/L,氢氧化钠1~6g/L,以0.5~2℃/min的升温速度升温至40~80℃,保温10~50min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:10~100投入染浴中,以0.5~3℃/min的升温速度升温至20~60℃,保温30~60min;最后将染色织物水洗、皂洗、水洗、烘干或晾干。
所述步骤(1)中的载体为苯甲醇、LEVEGAL®PEW-T(拓纳化学荷兰公司)或JYK POW(上海洁宜康化工科技有限公司)。
所述步骤(1)中载体的用量为1~30g/L。
所述步骤(1)中氯化钠的用量为1~50g/L。
本发明的有益效果:本发明在涤棉织物靛蓝染料染色浴中加入降低涤纶染色温度的载体,降低了涤纶染色温度,避免了靛蓝染料高温条件下结构发生变化,使上染涤棉织物的靛蓝从织物上解吸的问题;采用了两浴两步染色法对涤棉织物进行染色,使涤纶和棉织物有较好的同色性且达到满意的染色深度。本发明的技术方案工艺简单可行,对靛蓝染料和织物织造过程无特殊要求,利用常见印染厂染色设备就可达规模生产,具有广阔的应用前景。
具体实施方式
实施例1
一种涤棉织物靛蓝染料同色染色的方法,其过程如下:用靛蓝染料对涤棉织物进行两浴两步染色,第一步染色时染浴中加入靛蓝染料、保险粉、氢氧化钠,上述溶液以1℃/min的升温速度升温至60℃,保温30min使靛蓝染料还原,然后在上述还原液中加入载体苯甲醇和氯化钠,将涤棉织物(采用纯涤纶和涤棉织物按照质量比为1:1进行染色,以比较其同色性)按浴比1:30投入上述溶液中,以2℃/min的升温速度升温至100℃,保温40min;第二步染色时染浴中加入靛蓝染料、保险粉和氢氧化钠,上述溶液以1.5 ℃/min的升温速度升温至60℃,保温30min使靛蓝染料还原,将第一步染色后的涤棉织物按浴比1:50投入上述溶液中, 60℃保温40min;最后将染色织物用冷水充分洗涤,再用2g/L标准合成洗涤剂和2g/L纯碱于80℃洗涤15min,然后用冷水充分洗涤、烘干或晾干。
第一步染色时染液处方1如下:
靛蓝染料 2% owf
保险粉 10 g/L
氢氧化钠 3 g/L
载体苯甲醇 20 g/L
氯化钠 10 g/L
第二步染色时染液处方2如下:
靛蓝染料 4% owf
保险粉 15g/L
氢氧化钠 4g/L
实施例2
一种涤棉牛仔面料的制备方法,其过程如下:用靛蓝染料对涤棉织物进行两浴两步染色,第一步染色时染浴中加入靛蓝染料、保险粉、氢氧化钠,上述溶液以2℃/min的升温速度升温至50℃,保温40min使靛蓝染料还原,然后在上述还原液中加入载体苯甲醇和氯化钠,将涤棉织物按浴比1:50投入上述溶液中,以1℃/min的升温速度升温至90℃,保温60min;第二步染色时染浴中加入靛蓝染料、保险粉和氢氧化钠,上述溶液以2 ℃/min的升温速度升温至50℃,保温30min使靛蓝染料还原,将第一步染色后的涤棉织物按浴比1:50投入上述溶液中,50℃保温60min;最后将染色织物用冷水充分洗涤,再用2g/L标准合成洗涤剂和2g/L纯碱于80℃洗涤15min,然后用冷水充分洗涤、烘干或晾干。
第一步染色时染液处方1如下:
靛蓝染料 1% owf
保险粉 8 g/L
氢氧化钠 2 g/L
载体苯甲醇 30 g/L
氯化钠 30 g/L
第二步染色时染液处方2如下:
靛蓝染料 6% owf
保险粉 13 g/L
氢氧化钠 6 g/L
实施例3
一种涤棉牛仔面料的制备方法,其过程如下:用靛蓝染料对涤棉织物进行两浴两步染色,第一步染色时染浴中加入靛蓝染料、保险粉、氢氧化钠,上述溶液以1℃/min的升温速度升温至40℃,保温30min使靛蓝染料还原,然后在上述还原液中加入载体JYK POW和氯化钠,将涤棉织物按浴比1:20投入上述溶液中,以1.5℃/min的升温速度升温至85℃,保温45min;第二步染色时染浴中加入靛蓝染料、保险粉和氢氧化钠,上述溶液以1 ℃/min的升温速度升温至40℃,保温30min使靛蓝染料还原,将第一步染色后的涤棉织物按浴比1:15投入上述溶液中,40℃保温50min;最后将染色织物用冷水充分洗涤,再用2g/L标准合成洗涤剂和2g/L纯碱于80℃洗涤15min,然后用冷水充分洗涤、烘干或晾干。
第一步染色时染液处方1如下:
靛蓝染料 0.5 % owf
保险粉 4 g/L
氢氧化钠 2 g/L
载体JYK POW 18 g/L
氯化钠 20 g/L
第二步染色时染液处方2如下:
靛蓝染料 5% owf
保险粉 10 g/L
氢氧化钠 5 g/L
实施例4
一种涤棉牛仔面料的制备方法,其过程如下:用靛蓝染料对涤棉织物进行两浴两步染色,第一步染色时染浴中加入靛蓝染料、保险粉、氢氧化钠,上述溶液以2℃/min的升温速度升温至50℃,保温20min使靛蓝染料还原,然后在上述还原液中加入载体LEVEGAL®PEW-T和氯化钠,将涤棉织物按浴比1:60投入上述溶液中,以2℃/min的升温速度升温至95℃,保温25min;第二步染色时染浴中加入靛蓝染料、保险粉和氢氧化钠,上述溶液以2 ℃/min的升温速度升温至50℃,保温20min使靛蓝染料还原,再将还原液降温至30℃,然后将第一步染色后的涤棉织物按浴比1:25投入上述溶液中,30℃保温60min;最后将染色织物用冷水充分洗涤,再用2g/L标准合成洗涤剂和2g/L纯碱于80℃洗涤15min,然后用冷水充分洗涤、烘干或晾干。
第一步染色时染液处方1如下:
靛蓝染料 4 % owf
保险粉 16 g/L
氢氧化钠 6 g/L
载体LEVEGAL®PEW-T 12 g/L
氯化钠 5 g/L
第二步染色时染液处方2如下:
靛蓝染料 6% owf
保险粉 20 g/L
氢氧化钠 6 g/L
实施例5
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料0.05%owf,保险粉2g/L,氢氧化钠8g/L,以0.5℃/min的升温速度升温至40℃,保温50min使靛蓝染料还原,然后加入载体苯甲醇1g/L和氯化钠50g/L,将涤棉织物按浴比1:10投入染浴中,以0.5℃/min的升温速度升温至80℃,保温90min;
(2)在另一个染浴中加入靛蓝染料0.5%owf,保险粉40g/L,氢氧化钠1g/L,以0.5℃/min的升温速度升温至40℃,保温50min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:10投入染浴中,以0.5℃/min的升温速度升温至20℃,保温60min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
实施例6
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料8%owf,保险粉50g/L,氢氧化钠0.5g/L,以2℃/min的升温速度升温至80℃,保温10min使靛蓝染料还原,然后加入载体LEVEGAL®PEW-T(拓纳化学荷兰公司)30g/L和氯化钠1g/L,将涤棉织物按浴比1: 100投入染浴中,以3℃/min的升温速度升温至100℃,保温20min;
(2)在另一个染浴中加入靛蓝染料6%owf,保险粉3g/L,氢氧化钠6g/L,以2℃/min的升温速度升温至80℃,保温10min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:100投入染浴中,以3℃/min的升温速度升温至60℃,保温30min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
实施例7
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料5%owf,保险粉25g/L,氢氧化钠1g/L,以1℃/min的升温速度升温至50℃,保温30min使靛蓝染料还原,然后加入载体JYK POW(上海洁宜康化工科技有限公司)15g/L和氯化钠40g/L,将涤棉织物按浴比1:20投入染浴中,以1℃/min的升温速度升温至85℃,保温80min;
(2)在另一个染浴中加入靛蓝染料1%owf,保险粉5g/L,氢氧化钠2g/L,以1℃/min的升温速度升温至50℃,保温30min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:20投入染浴中,以1℃/min的升温速度升温至30℃,保温50min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
实施例8
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料0.1%owf,保险粉40g/L,氢氧化钠4g/L,以1.5℃/min的升温速度升温至60℃,保温20min使靛蓝染料还原,然后加入载体苯甲醇2g/L和氯化钠4g/L,将涤棉织物按浴比1:50投入染浴中,以2℃/min的升温速度升温至90℃,保温30min;
(2)在另一个染浴中加入靛蓝染料2%owf,保险粉20g/L,氢氧化钠3g/L,以1.5℃/min的升温速度升温至70℃,保温20min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:50投入染浴中,以2.5℃/min的升温速度升温至40℃,保温40min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
实施例9
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料3%owf,保险粉30g/L,氢氧化钠7g/L,以1.5℃/min的升温速度升温至70℃,保温40min使靛蓝染料还原,然后加入载体苯甲醇5g/L和氯化钠2g/L,将涤棉织物按浴比1:80投入染浴中,以2.5℃/min的升温速度升温至95℃,保温80min;
(2)在另一个染浴中加入靛蓝染料3%owf,保险粉3.5g/L,氢氧化钠2.5g/L,以2℃/min的升温速度升温至50℃,保温45min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:70投入染浴中,以1.5℃/min的升温速度升温至30℃,保温50min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
实施例10
本实施例的涤棉织物靛蓝染料同色染色的方法,用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料7%owf,保险粉45g/L,氢氧化钠5g/L,以2min的升温速度升温至60℃,保温20min使靛蓝染料还原,然后加入载体苯甲醇10g/L和氯化钠8g/L,将涤棉织物按浴比1:60投入染浴中,以3℃/min的升温速度升温至85℃,保温40min;
(2)在另一个染浴中加入靛蓝染料4.5%owf,保险粉30g/L,氢氧化钠4.5g/L,以2.5℃/min的升温速度升温至70℃,保温15min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:80投入染浴中,以2.5℃/min的升温速度升温至45℃,保温35min;保温结束染色织物先用冷水洗涤,再用温水洗涤,然后进行皂洗(皂洗剂LTS 2g/L,90℃洗涤10min),皂洗结束再用冷水和温水洗涤,然后将织物进行烘干或晾干。
本发明的实施效果
涤棉织物分别经实施例1~10染色处理后,对其进行如下测试,测试结果见表1。
1)K/S值(表观颜色深度)
在UltraScan PRO测色仪(美国HunterLab公司)上测定,采用D65光源和10°观察角观察。
2)同色性指数K值
同色性指数按以下公式计算:
式中,K为同色性指数,K值越趋近于1说明染色涤棉织物的同色性越好。
3)染色织物的牢度
依据GB/T 3921-2008和GB/T 3920-2008分别测试织物的耐洗牢度和耐摩擦牢度。
由表1可知,染色涤纶和棉织物具有较高的表观颜色深度,且同色性指数K值均趋近于1,说明染色织物可获得良好的同色性。染色织物的摩擦牢度均达3级以上,皂洗牢度牢度均达4级以上。由此可见,本发明所提供的技术方案能够赋予涤棉织物较好的同色性、较深的颜色和良好的耐洗和耐摩擦牢度。
表1 实施染色涤棉织物的测试结果

Claims (3)

1.一种涤棉织物靛蓝染料同色染色的方法,其特征在于:用靛蓝染料对涤棉织物进行两浴两步染色,步骤如下:
(1)在染浴中加入靛蓝染料0.05~8%owf,保险粉2~50g/L,氢氧化钠0.5~8g/L,以0.5~2℃/min的升温速度升温至40~80℃,保温10~50min使靛蓝染料还原,然后加入载体和氯化钠,将涤棉织物按浴比1:10~100投入染浴中,以0.5~3℃/min的升温速度升温至80~100℃,保温20~90min;
(2)在另一个染浴中加入靛蓝染料0.5~6%owf,保险粉3~40g/L,氢氧化钠1~6g/L,以0.5~2℃/min的升温速度升温至40~80℃,保温10~50min使靛蓝染料还原,将步骤(1)染色后的涤棉织物按浴比1:10~100投入染浴中,以0.5~3℃/min的升温速度升温至20~60℃,保温30~60min;最后将染色织物水洗、皂洗、水洗、烘干或晾干;所述步骤(1)中载体的用量为1~30g/L。
2.根据权利要求1所述的涤棉织物靛蓝染料同色染色的方法,其特征在于:所述步骤(1)中的载体为苯甲醇、LEVEGAL®PEW-T或JYK POW。
3.根据权利要求1所述的涤棉织物靛蓝染料同色染色的方法,其特征在于:所述步骤(1)中氯化钠的用量为1~50g/L。
CN201410256555.2A 2014-06-10 2014-06-10 一种涤棉织物靛蓝染料同色染色的方法 Expired - Fee Related CN104088173B (zh)