CN103694577B - 一种耐氧化电容器橡胶密封圈及其制备方法 - Google Patents

一种耐氧化电容器橡胶密封圈及其制备方法 Download PDF

Info

Publication number
CN103694577B
CN103694577B CN201310648397.0A CN201310648397A CN103694577B CN 103694577 B CN103694577 B CN 103694577B CN 201310648397 A CN201310648397 A CN 201310648397A CN 103694577 B CN103694577 B CN 103694577B
Authority
CN
China
Prior art keywords
rubber
antioxidant
mixing
rubber seal
resistance
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201310648397.0A
Other languages
English (en)
Other versions
CN103694577A (zh
Inventor
连秉卫
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nantong Yaohua Fibre Co ltd
Original Assignee
TONGLING RIXING ELECTRONICS Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TONGLING RIXING ELECTRONICS Co Ltd filed Critical TONGLING RIXING ELECTRONICS Co Ltd
Priority to CN201310648397.0A priority Critical patent/CN103694577B/zh
Publication of CN103694577A publication Critical patent/CN103694577A/zh
Application granted granted Critical
Publication of CN103694577B publication Critical patent/CN103694577B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种耐氧化电容器橡胶密封圈,其特征在于,由下列重量份的原料制成:氯醇橡胶(T3100)10-15、三元乙丙橡胶(德国朗盛9650)60-62、氧化锌2-3、硬脂酸3-4、防老剂4010?1-2、石棉粉3-4、聚磷酸铵2-3、N220炭黑30-35、轻质碳酸钙15-18、防老剂4010?1-3、硫磺0.3-0.5、促进剂TMTD1-1.2、氧化镁1-2、改性凹凸棒土12-15;本发明添加改性凹凸棒土,改善了胶料的工艺性能,使用环保型配合剂,减少其毒副作用和对环境的污染;本发明橡胶密封圈具有良好的耐氧化性能,经久耐用,而且具有良好的耐油性,成本低。

Description

一种耐氧化电容器橡胶密封圈及其制备方法
技术领域
本发明涉及橡胶复合材料加工领域,特别是一种耐氧化电容器橡胶密封圈及其制备方法。
背景技术
电容器通常简称为电容,是电子设备中大量使用的电子元件之一,广泛应用于电路的隔直通交、耦合、旁路、滤波、调谐回路、能量转换、控制等方面。电容器由壳体、电容芯子、端盖及接线端子组成,电容器壳体内装有浸渍介质,浸渍介质一般为植物油或矿物油,电容器的密封部位均设有密封垫或密封圈,由于电容器的工作环境千差万别,有的电容器需要在恶劣的环境下工作,电容器密封垫需要耐高温、耐寒、耐酸碱、耐盐雾等有不同要求。
发明内容
本发明的目的是提供一种耐氧化电容器橡胶密封圈及其制备方法。
为了实现本发明的目的,本发明通过以下方案实施:
一种耐氧化电容器橡胶密封圈,由下列重量份的原料制成:氯醇橡胶(T3100)10-15、三元乙丙橡胶(德国朗盛9650)60-62、、氧化锌2-3、硬脂酸3-4、防老剂40101-2、石棉粉3-4、聚磷酸铵2-3、N220炭黑30-35、轻质碳酸钙15-18、防老剂40101-3、硫磺0.3-0.5、促进剂TMTD1-1.2、氧化镁1-2、改性凹凸棒土12-15;
所述改性凹凸棒土由下列重量份的原料制成:凹凸棒土20-24、甲苯二异氰酸酯3-4、二缩三丙二醇二丙烯酸酯2-3、粘土12-15、纳米二氧化钛3-4、氟化锆1-2、甲基三乙氧基硅烷1-2、二茂铁1-2、促进剂TMTD1-2、氢氧化铝8-10、2-氨基-2-甲基-1-丙醇2-3、花椒籽油1-2;制备方法是将凹凸棒土、粘土混合放入煅烧炉中在700-720℃下煅烧3-4小时,冷却,放入10-12%盐酸溶液中浸泡1-2小时,过滤取出,用清水洗净烘干,粉碎成200-300目粉末,与其它剩余成分混合,研磨分散1-2小时,即得。
本发明所述耐氧化电容器橡胶密封圈,由以下具体步骤制成:将三元乙丙橡胶(德国朗盛9650)、、氧化锌、硬脂酸、防老剂4010加入密炼机中,加热至80-85℃,混炼3-5min;然后升温至130-150℃,再加入轻质碳酸钙、防老剂4010、硫磺、促进剂TMTD,混炼6-8min,再加入石棉粉、聚磷酸铵、N220炭黑继续混炼4-6min,加入其余剩余成分混炼6-8min,即得本发明橡胶料。
本发明的优异效果是:本发明添加改性凹凸棒土,改善了胶料的工艺性能,使用环保型配合剂,减少其毒副作用和对环境的污染;本发明橡胶密封圈具有良好的耐氧化性能,经久耐用,而且具有良好的耐油性,成本低。
具体实施方式
下面通过具体实例对本发明进行详细说明。
一种耐氧化电容器橡胶密封圈,由下列重量份(公斤)的原料制成:氯醇橡胶(T3100)10、三元乙丙橡胶(德国朗盛9650)60、氧化锌2、硬脂酸3、防老剂40101、石棉粉3、聚磷酸铵2、N220炭黑30、轻质碳酸钙15、防老剂40101、硫磺0.3、促进剂TMTD1、氧化镁1、改性凹凸棒土12;
所述改性凹凸棒土由下列重量份(公斤)的原料制成:凹凸棒土20、甲苯二异氰酸酯3、二缩三丙二醇二丙烯酸酯2、粘土12、纳米二氧化钛3、氟化锆1、甲基三乙氧基硅烷1、二茂铁1、促进剂TMTD1、氢氧化铝8、2-氨基-2-甲基-1-丙醇2、花椒籽油1;制备方法是将凹凸棒土、粘土混合放入煅烧炉中在700-720℃下煅烧3-4小时,冷却,放入10-12%盐酸溶液中浸泡1-2小时,过滤取出,用清水洗净烘干,粉碎成200-300目粉末,与其它剩余成分混合,研磨分散1-2小时,即得。本发明所述耐氧化电容器橡胶密封圈,由以下具体步骤制成:将三元乙丙橡胶(德国朗盛9650)、、氧化锌、硬脂酸、防老剂4010加入密炼机中,加热至80-85℃,混炼3-5min;然后升温至130-150℃,再加入轻质碳酸钙、防老剂4010、硫磺、促进剂TMTD,混炼6-8min,再加入石棉粉、聚磷酸铵、N220炭黑继续混炼4-6min,加入其余剩余成分混炼6-8min,即得本发明橡胶料。
用本发明的耐腐蚀橡胶密封圈与普通胶料物理性能对比如下表。
从表中可以看出用本发明的橡胶密封圈产品,综合性能比较好。

Claims (2)

1.一种耐氧化电容器橡胶密封圈,其特征在于,由下列重量份的原料制成:氯醇橡胶10-15、三元乙丙橡胶60-62、氧化锌2-3、硬脂酸3-4、防老剂40101-2、石棉粉3-4、聚磷酸铵2-3、N220炭黑30-35、轻质碳酸钙15-18、防老剂40101-3、硫磺0.3-0.5、促进剂TMTD1-1.2、氧化镁1-2、改性凹凸棒土12-15;所述改性凹凸棒土由下列重量份的原料制成:凹凸棒土20-24、甲苯二异氰酸酯3-4、二缩三丙二醇二丙烯酸酯2-3、粘土12-15、纳米二氧化钛3-4、氟化锆1-2、甲基三乙氧基硅烷1-2、二茂铁1-2、促进剂TMTD1-2、氢氧化铝8-10、2-氨基-2-甲基-1-丙醇2-3、花椒籽油1-2;所述改性凹凸棒土的制备方法是将凹凸棒土、粘土混合放入煅烧炉中在700-720℃下煅烧3-4小时,冷却,放入10-12%盐酸溶液中浸泡1-2小时,过滤取出,用清水洗净烘干,粉碎成200-300目粉末,与其它剩余成分混合,研磨分散1-2小时,即得。
2.根据权利要求1所述耐氧化电容器橡胶密封圈,其特征在于,由以下具体步骤制成:将三元乙丙橡胶、氧化锌、硬脂酸、防老剂4010加入密炼机中,加热至80-85℃,混炼3-5min;然后升温至130-150℃,再加入轻质碳酸钙、防老剂4010、硫磺、促进剂TMTD,混炼6-8min,再加入石棉粉、聚磷酸铵、N220炭黑继续混炼4-6min,加入其余剩余成分混炼6-8min,即得本发明橡胶料。
CN201310648397.0A 2013-12-04 2013-12-04 一种耐氧化电容器橡胶密封圈及其制备方法 Active CN103694577B (zh)