CN103352215A - 一种工件的磷化防锈处理工艺 - Google Patents

一种工件的磷化防锈处理工艺 Download PDF

Info

Publication number
CN103352215A
CN103352215A CN2013102490782A CN201310249078A CN103352215A CN 103352215 A CN103352215 A CN 103352215A CN 2013102490782 A CN2013102490782 A CN 2013102490782A CN 201310249078 A CN201310249078 A CN 201310249078A CN 103352215 A CN103352215 A CN 103352215A
Authority
CN
China
Prior art keywords
workpiece
oil
treatment process
add
phosphorization
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2013102490782A
Other languages
English (en)
Other versions
CN103352215B (zh
Inventor
胡磊
耿良照
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
The following Electromechanical Technology Co., Ltd in Anhui
Original Assignee
Anhui Liu'an Zhaohui Machinery Manufacturing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Anhui Liu'an Zhaohui Machinery Manufacturing Co Ltd filed Critical Anhui Liu'an Zhaohui Machinery Manufacturing Co Ltd
Priority to CN201310249078.2A priority Critical patent/CN103352215B/zh
Publication of CN103352215A publication Critical patent/CN103352215A/zh
Application granted granted Critical
Publication of CN103352215B publication Critical patent/CN103352215B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种工件的磷化防锈处理工艺,包括以下步骤:(1)除油(2)除锈(3)磷化(4)水洗(5)烘干(6)防锈处理(7)卸料、包装。本发明的表面磷化防锈处理工艺易操作,用时短,使用的防锈油不易氧化,不影响工件的外观,综合性能优异,在工件表面铺展性能好,形成的油膜均匀稳定,极大的提高了对金属的保护作用。

Description

一种工件的磷化防锈处理工艺
技术领域
    本发明主要涉及一种工件处理工艺,尤其涉及一种工件的磷化防锈处理工艺。
背景技术
    磷化(phosphorization)是一种化学与电化学反应形成磷酸盐化学转化膜的过程,所形成的磷酸盐转化膜称之为磷化膜。磷化的目的主要是:给基体金属提供保护,在一定程度上防止金属被腐蚀;用于涂漆前打底,提高漆膜层的附着力与防腐蚀能力;在金属冷加工工艺中起减摩润滑使用。 磷化处理工艺应用于工业己有90多年的历史,大致可以分为三个时期:奠定磷化技术基础时期、磷化技术迅速发展时期和广泛应用时期,为了防止金属腐蚀的普遍做法是将工件表面涂上一层防锈油。
发明内容
本发明目的就是提供一种工件的磷化防锈处理工艺。
本发明是通过以下技术方案实现的:
一种工件的磷化防锈处理工艺,包括以下步骤:
(1)除油:先把工件放到电解槽内脱脂,除油温度90-100℃,时间20-30min;(2)除锈:浓度为3-5%的盐酸处理,时间3-5min;
(3)磷化:在磷化液内浸泡,时间10-15min,所述的每升磷化液溶液中所含原料重量(g)为:
磷酸二氢锌80-90、磷酸锰30-40、磷酸钙10-15、硫酸镍3-6、酒石酸2-4,剩余的为水;
(4)水洗:普通自来水,水洗干净;
(5)烘干:在烘箱中烘干,温度100-130℃,时间5-10min;
(6)防锈处理:在防锈油中浸泡2-3min,所述的防锈油是由下述重量份的原料组成的:
煤油60-70、150SN基础油20-30、液化石蜡3-4、2,6- 二叔丁基对甲酚1-2、硬脂酸2-3、松香2-3、硫代二丙酸二月桂酯1-2、甲基苯并三氮唑1-2、纳米碳粉0.2-0.4、十二烷基聚氧乙烯醚1-2、油酸聚氧乙烯酯2-3、eva树脂3-4、六次甲基四胺0.2-0.3;
所述的防锈油的制备包括以下步骤:
将上述煤油、150SN基础油加入到反应釜中,混合搅拌,加热到110-120℃,加入液化石蜡,充分搅拌;将上述松香加热溶解后加入eva树脂、十二烷基聚氧乙烯醚,常温搅拌10-15分钟,加入液体石蜡,低速300-500转/分分散6-10分钟,得预混料,将预混料加入到上述反应釜中,再加入甲基苯并三氮唑,连续脱水1-2小时,降温至于55-60℃;加入剩余各原料,充分搅拌,降低温度至35-38℃,过滤出料,即得所述防锈油;
(7)卸料、包装。
一种工件的磷化防锈处理工艺,所述的工件为碳钢或者合金钢。
本发明的优点是:
    本发明的表面磷化防锈处理工艺易操作,用时短,使用的防锈油不易氧化,不影响工件的外观,综合性能优异,在工件表面铺展性能好,形成的油膜均匀稳定,极大的提高了对金属的保护作用。
具体实施方式
实施例1
一种工件的磷化防锈处理工艺,包括以下步骤:
(1)除油:先把工件放到电解槽内脱脂,除油温度100℃,时间30min;(2)除锈:浓度为5%的盐酸处理,时间5min;
(3)磷化:在磷化液内浸泡,时间15min,所述的每升磷化液溶液中所含原料重量(g)为:
磷酸二氢锌90、磷酸锰40、磷酸钙15、硫酸镍3、酒石酸4,剩余的为水;
(4)水洗:普通自来水,水洗干净;
(5)烘干:在烘箱中烘干,温度130℃,时间10min;
(6)防锈处理:在防锈油中浸泡3min,所述的防锈油是由下述重量份的原料组成的:
煤油70、150SN基础油30、液化石蜡4、2,6- 二叔丁基对甲酚2、硬脂酸3、松香3、硫代二丙酸二月桂酯2、甲基苯并三氮唑2、纳米碳粉0.4、十二烷基聚氧乙烯醚2、油酸聚氧乙烯酯3、eva树脂4、六次甲基四胺0.3;
所述的防锈油的制备包括以下步骤:
将上述煤油、150SN基础油加入到反应釜中,混合搅拌,加热到120℃,加入液化石蜡,充分搅拌;将上述松香加热溶解后加入eva树脂、十二烷基聚氧乙烯醚,常温搅拌15分钟,加入液体石蜡,低速500转/分分散10分钟,得预混料,将预混料加入到上述反应釜中,再加入甲基苯并三氮唑,连续脱水1小时,降温至于60℃;加入剩余各原料,充分搅拌,降低温度至38℃,过滤出料,即得所述防锈油;
(7)卸料、包装。
一种工件的磷化防锈处理工艺,所述的工件为碳钢或者合金钢。

Claims (2)

1.一种工件的磷化防锈处理工艺,其特征在于包括以下步骤:
(1)除油:先把工件放到电解槽内脱脂,除油温度90-100℃,时间20-30min;(2)除锈:浓度为3-5%的盐酸处理,时间3-5min;
(3)磷化:在磷化液内浸泡,时间10-15min,所述的每升磷化液溶液中所含原料重量(g)为:
磷酸二氢锌80-90、磷酸锰30-40、磷酸钙10-15、硫酸镍3-6、酒石酸2-4,剩余的为水;
(4)水洗:普通自来水,水洗干净;
(5)烘干:在烘箱中烘干,温度100-130℃,时间5-10min;
(6)防锈处理:在防锈油中浸泡2-3min,所述的防锈油是由下述重量份的原料组成的:
煤油60-70、150SN基础油20-30、液化石蜡3-4、2,6- 二叔丁基对甲酚1-2、硬脂酸2-3、松香2-3、硫代二丙酸二月桂酯1-2、甲基苯并三氮唑1-2、纳米碳粉0.2-0.4、十二烷基聚氧乙烯醚1-2、油酸聚氧乙烯酯2-3、eva树脂3-4、六次甲基四胺0.2-0.3;
所述的防锈油的制备包括以下步骤:
将上述煤油、150SN基础油加入到反应釜中,混合搅拌,加热到110-120℃,加入液化石蜡,充分搅拌;将上述松香加热溶解后加入eva树脂、十二烷基聚氧乙烯醚,常温搅拌10-15分钟,加入液体石蜡,低速300-500转/分分散6-10分钟,得预混料,将预混料加入到上述反应釜中,再加入甲基苯并三氮唑,连续脱水1-2小时,降温至于55-60℃;加入剩余各原料,充分搅拌,降低温度至35-38℃,过滤出料,即得所述防锈油;
(7)卸料、包装。
2.根据权利要求1所述的一种工件的磷化防锈处理工艺,其特征在于所述的工件为碳钢或者合金钢。
CN201310249078.2A 2013-06-21 2013-06-21 一种工件的磷化防锈处理工艺 Active CN103352215B (zh)