CN103333557A - 糯米粉环保水性涂料 - Google Patents

糯米粉环保水性涂料 Download PDF

Info

Publication number
CN103333557A
CN103333557A CN 201310250355 CN201310250355A CN103333557A CN 103333557 A CN103333557 A CN 103333557A CN 201310250355 CN201310250355 CN 201310250355 CN 201310250355 A CN201310250355 A CN 201310250355A CN 103333557 A CN103333557 A CN 103333557A
Authority
CN
China
Prior art keywords
minutes
rice flour
water
paint
based paint
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 201310250355
Other languages
English (en)
Inventor
罗家斌
黄定华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
DONGGUAN DR HEALTHY WOOD GLUE Co Ltd
Original Assignee
DONGGUAN DR HEALTHY WOOD GLUE Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by DONGGUAN DR HEALTHY WOOD GLUE Co Ltd filed Critical DONGGUAN DR HEALTHY WOOD GLUE Co Ltd
Priority to CN 201310250355 priority Critical patent/CN103333557A/zh
Publication of CN103333557A publication Critical patent/CN103333557A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种涂料,尤其是涉及一种环保无毒无害生物质涂料。按质量份数计由以下组成:水10-25%、纤维素2-5%、润湿剂1-4%、消泡剂1-4%、钛白粉10-30%、碳酸钙15-40%、VAE15-35%、糯米粉10-15%、石灰浆清液5-10%、纳米银0.5-1%。采用上述技术方案,配方中的糯米粉和碳酸钙,生石灰混合使用,生成一种有机—无机复合材料,这种材料结构致密,力学强度高。韧性好,对基材密封好,因此,得到的涂料耐候性、耐老化性极佳,同时添加植物提取液,使涂膜更清新自然,不含有害成分、安全环保、制作简单。

Description

糯米粉环保水性涂料
技术领域
本发明涉及一种涂料,尤其是涉及一种环保无毒无害生物质涂料。
背景技术
现有的水性乳胶涂涂料基本都是含有甲醛、苯、甲苯,VOC等对人体有毒有害的成份,在使用该产品后,有害物质会隐藏其中,慢慢挥发,甚至于要三到十五年。对人体有着很大的危害,而且在生产制造,使用过程中均会对环境造成污染,还会对使用者的健康造成严重伤害。
申请人之前申请了有关“多功能糯米涂料”的专利,该申请的配方在工艺实施过程中,操作繁琐,尤其是糯米浆液的使用不好把握,再加上我国南方区域潮湿多雨,糯米浆液的生产、保管、储存都有众多的困难。而导致最终产品的质量出现问题。
发明内容
为了克服上述现有的技术缺陷,本发明提供了一种工艺简单,操作简便,高耐候,高粘接强调的水性涂料。
本发明采用的技术方案是:糯米粉环保水性涂料,按质量份数计由以下组成:
Figure BDA00003388319900011
上述所述石灰浆清液将生石灰加入水中搅拌30分钟,澄清后取上部溶液为石灰浆清液;
上述所述VAE为聚醋酸乙烯-乙烯乳液。
上述的糯米粉环保水性涂料,按质量份数计由以下组成:
Figure BDA00003388319900021
上述的糯米粉环保水性涂料的制作方法,包括如下步骤:
①将纤维素加入水中搅拌30分钟;
②依次加入润湿剂,消泡剂搅拌30分钟;
③加入钛白粉,超细碳酸钙强力分散30分钟;
④加入食品级VAE,糯米粉搅拌20分钟;
⑤加入石灰浆清液搅拌20分钟;
⑥加入纳米银,搅拌20分钟;
⑦过滤包装。
采用上述技术方案,配方中的糯米粉和碳酸钙,生石灰混合使用,生成一种有机——无机复合材料,这种材料结构致密,力学强度高。韧性好,对基材密封好,因此,得到的涂料耐候性、耐老化性极佳,同时添加植物提取液,使涂膜更清新自然,不含有害成分、安全环保、制作简单。
具体实施方式
实施例一:
首先,将生石灰加入水中搅拌30分钟,澄清后取上部溶液为石灰浆清液,待用。
按照以下配方(按质量份数计)、以下步骤操作:
Figure BDA00003388319900022
Figure BDA00003388319900031
①将羟丙基甲基纤维素加入水中搅拌30分钟;
②依次加入聚羧酸钠盐分散剂、有机硅消泡剂搅拌30分钟;
③加入钛白粉、超细碳酸钙强力分散30分钟;
④加入聚醋酸乙烯-乙烯乳液、糯米粉搅拌20分钟;
⑤加入石灰浆搅拌20分钟;
⑥加入纳米银,搅拌20分钟;
⑦过滤后成为本发明涂料成品,进行包装。
所述羟丙基甲基纤维素,简称:UPMC,其产地为美国,生产厂商为亚什兰ASHLAND。
所述聚羧酸钠盐分散剂,简称:SN-5040,其产地为日本,生产商为诺普科公司。
所述有机硅消泡剂,简称:DREWPLUS2101EFG,其产地为美国,生产厂商为亚什兰ASHLAND。
所述聚醋酸乙烯-乙烯乳液,其生产厂家为德国瓦克公司。
采用此配方,生产10批次的涂料,其主要技术指标都在下表范围内:
pH值 粘度 附着力 固含量 耐洗刷
7-8 100±5ku ≥98% 55±2% ≥50000次
实施例二:
首先,将生石灰加入水中搅拌30分钟,澄清后取上部溶液为石灰浆清液,待用。
按照以下配方(按质量份数计)、以下步骤操作:
Figure BDA00003388319900032
Figure BDA00003388319900041
采用此配方,按照实施例一的生产方法生产10批次的涂料,其主要技术指标都在下表范围内:
pH值 粘度 附着力 固含量 耐洗刷
7-8 100±5ku ≥99% 55±2% ≥55000次
实施例三:
首先,将生石灰加入水中搅拌30分钟,澄清后取上部溶液为石灰浆清液,待用。
按照以下配方(按质量份数计)、以下步骤操作:
Figure BDA00003388319900042
采用此配方,按照实施例一的生产方法生产10批次的涂料,其主要技术指标都在下表范围内:
pH值 粘度 附着力 固含量 耐洗刷
7-8 100±5ku ≥98% 55±2% ≥50000次

Claims (3)

1.糯米粉环保水性涂料,其特征在于按质量份数计包括:
Figure FDA00003388319800011
上述所述石灰浆清液将生石灰加入水中搅拌30分钟,澄清后取上部溶液为石灰浆清液;
上述所述VAE为聚醋酸乙烯-乙烯乳液。
2.根据权利要求1所述的糯米粉环保水性涂料,其特征在于按质量份数计由以下组成:
Figure FDA00003388319800012
3.权利要求1所述的糯米粉环保水性涂料的制作方法,包括如下步骤:
①将纤维素加入水中搅拌30分钟;
②依次加入润湿剂、消泡剂搅拌30分钟;
③加入钛白粉、碳酸钙强力分散30分钟;
④加入食品级VAE、糯米粉搅拌20分钟;
⑤加入石灰浆清液搅拌20分钟;
⑥加入纳米银搅拌20分钟;
⑦过滤包装。
CN 201310250355 2013-06-21 2013-06-21 糯米粉环保水性涂料 Pending CN103333557A (zh)