CN103318853A - 一种回收铜阳极泥中硒的方法 - Google Patents
一种回收铜阳极泥中硒的方法 Download PDFInfo
- Publication number
- CN103318853A CN103318853A CN2013102386399A CN201310238639A CN103318853A CN 103318853 A CN103318853 A CN 103318853A CN 2013102386399 A CN2013102386399 A CN 2013102386399A CN 201310238639 A CN201310238639 A CN 201310238639A CN 103318853 A CN103318853 A CN 103318853A
- Authority
- CN
- China
- Prior art keywords
- selenium
- copper
- copper anode
- anode slime
- reaction
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明公开了一种回收铜阳极泥中硒的方法,其特点是它包括如下工艺步骤:铜阳极泥加铜粉、浓硫酸浆化后送至回转窑焙烧,铜粉在焙烧时生成二氧化硫气体,生成的气体能够起到解决蓬松焙砂、破坏硫酸银、硫酸铅表面张力大问题,从而降低了焙砂粒度,既保证了铜阳极泥中硒的焙烧效果又满足了下道湿法工艺处理的要求;本工艺设备配置简单,尤其适用于复杂含高银、高铅、低铜的铜阳极泥的处理,操作稳定便于控制,资源综合利用率高。
Description
技术领域:
本方法属于冶金工艺技术领域,具体地讲是一种回收铜阳极泥中硒的方法,特别适用于复杂含高银、高铅、低铜的铜阳极泥的处理。
背景技术:
目前,铜阳极泥处理主要工艺为,阳极泥经浓硫酸浆化后直接回转窑焙烧,产出适合湿法工艺要求的焙砂;若含银量在25-30%,铅含量在20-28%的铜阳极泥经常规焙烧后产生的焙砂的粒度较大,通常呈块状;硒回收率极低,焙砂质量不能满足湿法处理的要求。
发明内容:
本发明的目的是克服上述已有技术的不足,而提供一种回收铜阳极泥中硒的方法,主要解决现有的工艺对银含量25-30%、铅含量20-28%的铜阳极泥硒回收率极低的问题。
本发明的技术方案是:一种回收铜阳极泥中硒的方法,其特殊之处在于它包括如下工艺步骤:
a将浓硫酸加入到反应釜中,浓硫酸与铜阳极泥的液固重量比为0.8-1.5:1,同时加入适量的铜粉,铜粉加入后使物料中含铜量10%,开启一次浆化6h,搅拌料浆成糊状;
b反应完成后,将料浆均匀投入回转窑中进行焙烧,料浆在窑内停留3-5h,焙砂流入料斗,反应产生的二氧化硫和二氧化硒进入吸收塔进行还原反应,产出粗硒;反应原理:
2H2SO4(浓)+Cu≜CuSO4+SO2+2H2O;
SeO2+H2O=H2SeO3;
H2SeO3+2SO2+H2O=2H2SO4+Se;
c将焙砂加入反应釜内,再加入水、浓硫酸搅拌;在85℃恒温下反应2h;过滤后,得到浸出后液和浸出渣;
d浸出后液通过氯化沉银、铁粉置换工艺得到银粉;
e浸出渣通过氯化分金、二氧化硫还原工艺得到金粉。
进一步,b步骤所述的回转窑包括干燥区和硒挥发区,干燥区温度300-350℃,硒挥发区温度450℃-530℃。
本发明的一种回收铜阳极泥中硒的方法,在焙烧处理前调整物料比例,以达到降低焙砂粒度,提高硒的回收率,并为后续工艺提取贵金属提供合适物料的目的。
本发明的一种回收铜阳极泥中硒的方法与已有技术相比具有突出的实质性特点和显著进步,1、由于在铜阳极泥中加入铜粉,铜粉在焙烧时生成二氧化硫气体,生成的气体能够起到解决蓬松焙砂、破坏硫酸银、硫酸铅表面张力大问题,从而降低了焙砂粒度,既保证了铜阳极泥中硒的焙烧效果又满足了下道湿法工艺处理的要求;2、工艺设备配置简单,操作稳定便于控制;3、资源综合利用率高,金、银、硒都得到了回收利用;4、回收成本低,具有很高的经济价值;5、有效的提高硒的回收率,降低焙砂的粒度。
具体实施方式:
为了更好地理解与实施,下面结合实施例详细说明本发明;所举实施例只用于解释本发明,并非用于限定本发明的范围。
实施例1:铜阳极泥以含有如下元素的为例,其元素含量如表1:
表1
名称 | 金 | 名称 | 银 |
含量(%) | 0.62 | 含量(%) | 26.89 |
名称 | 硒 | 名称 | 铜 |
含量(%) | 2.28 | 含量(%) | 3.07 |
名称 | 铅 | 名称 | 铂 |
含量(%) | 22.88 | 含量(g/t) | 14.98 |
名称 | 钯 | ||
含量(g/t) | 47.18 |
采取如下工艺步骤:
1、向浆化槽内加入浓硫酸(93%)1t,加入铜阳极泥(干重)1t,同时加入铜粉70kg,开启搅拌在常温下浆化6h,搅拌料浆成糊状;
2、将浆化后的铜阳极泥加入回转窑进行焙烧,回转窑干燥区:温度350℃,干燥1.5h,硒挥发区:温度450℃,持续1.5h,温度530℃,持续1.5h;硒挥发后气体通过负压系统进入硒吸收釜后,溶解在水中生成亚硒酸,再与二氧化硫反应生成硒沉淀,经过过滤槽过滤后得到硒产品17.47kg;从回转窑出口放出的粉状焙砂1250kg,送至铜银浸出;其反应原理如下:
2H2SO4(浓)+Cu≜CuSO4+SO2+2H2O;
SeO2+H2O=H2SeO3;
H2SeO3+2SO2+H2O=2H2SO4+Se;
3、将1250kg焙砂加入反应釜内,再加入7500L水、浓硫酸(93%)750L搅拌;在85℃恒温下反应2h;过滤后,得到浸出后液8000L,浸出渣750kg;
4、浸出后液通过氯化沉银、铁粉置换工艺得到银粉265kg;
5、浸出渣通过氯化分金、二氧化硫还原工艺得到金粉6.16kg。
上述案例与未加入铜粉在相同条件下金属回收率对比如表2
表2
焙砂粒度 | 硒回收率 | 金回收率 | 银回收率 | |
未加铜粉 | 块状 | 70% | 97.5 % | 96% |
加铜粉 | 粉末状 | 95.78% | 99.39% | 98.6% |
实施例2,将浓硫酸加入到反应釜中,根据情况浓硫酸与铜阳极泥的液固重量比为0.8-1.5:1,同时加入适量的铜粉,铜粉加入后使物料中含铜量10%,开启一次浆化6h,搅拌料浆成糊状;反应完成后,将料浆均匀投入回转窑中进行焙烧,回转窑的干燥区温度300-350℃,硒挥发区温度450℃-530℃,料浆在窑内停留3-5h,焙砂流入料斗,反应产生的二氧化硫和二氧化硒进入吸收塔进行还原反应,产出粗硒;将焙砂加入反应釜内,再加入水、浓硫酸搅拌;在85℃恒温下反应2h;过滤后,得到浸出后液和浸出渣;浸出后液通过氯化沉银、铁粉置换工艺得到银粉;浸出渣通过氯化分金、二氧化硫还原工艺得到金粉。
Claims (2)
1.一种回收铜阳极泥中硒的方法,其特征在于它包括如下工艺步骤:
a将浓硫酸加入到反应釜中,浓硫酸与铜阳极泥的液固重量比为0.8-1.5:1,同时加入适量的铜粉,铜粉加入后使物料中含铜量10%,开启一次浆化6h,搅拌料浆成糊状;
b反应完成后,将料浆均匀投入回转窑中进行焙烧,料浆在窑内停留3-5h,焙砂流入料斗,反应产生的二氧化硫和二氧化硒进入吸收塔进行还原反应,产出粗硒;反应原理:
2H2SO4(浓)+Cu≜CuSO4+SO2+2H2O;
SeO2+H2O=H2SeO3;
H2SeO3+2SO2+H2O=2H2SO4+Se;
c将焙砂加入反应釜内,再加入水、浓硫酸搅拌;在85℃恒温下反应2h;过滤后,得到浸出后液和浸出渣;
d浸出后液通过氯化沉银、铁粉置换工艺得到银粉;
e浸出渣通过氯化分金、二氧化硫还原工艺得到金粉。
2.根据权利要求1所述的一种回收铜阳极泥中硒的方法,其特征在于b步骤所述的回转窑包括干燥区和硒挥发区,干燥区温度300-350℃,硒挥发区温度450℃-530℃。