CN103113079A - 一种矿用水玻璃加固堵水材料 - Google Patents

一种矿用水玻璃加固堵水材料 Download PDF

Info

Publication number
CN103113079A
CN103113079A CN2013100477868A CN201310047786A CN103113079A CN 103113079 A CN103113079 A CN 103113079A CN 2013100477868 A CN2013100477868 A CN 2013100477868A CN 201310047786 A CN201310047786 A CN 201310047786A CN 103113079 A CN103113079 A CN 103113079A
Authority
CN
China
Prior art keywords
water
glass
component
glass reinforced
mining
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2013100477868A
Other languages
English (en)
Inventor
柏广峰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanxi Yubang New Power Science & Technology Co Ltd
Original Assignee
Shanxi Yubang New Power Science & Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanxi Yubang New Power Science & Technology Co Ltd filed Critical Shanxi Yubang New Power Science & Technology Co Ltd
Priority to CN2013100477868A priority Critical patent/CN103113079A/zh
Publication of CN103113079A publication Critical patent/CN103113079A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种矿用水玻璃加固堵水材料,由两种独立的A组份与B组份组成,其中所述A组份的原料按照重量百分数为:水玻璃A:51~99.9%,水玻璃B:0~50%,催化剂C:0.1~2%,增塑剂D:0~50%;其中所述B组份的原料按照重量百分数为:固化剂A:51~100%,固化剂B:0~50%,聚醚多元醇C:0~50%。本发明的矿用加固材料阻燃性高、反应热低、固化时间可调、环境水对反应基本无影响的效果,很大程度上提高了煤矿的生产的安全性。

Description

一种矿用水玻璃加固堵水材料
技术领域
本发明属于矿用加固堵水材料领域,具体涉及一种矿用水玻璃加固堵水材料。
背景技术
在矿山压力作用下及遇到地质断层、陷落柱时,巷道、工作面顶板煤体酥散,造成巷道变形,顶板冒落,煤帮片落,给安全生产带来隐患。
煤矿在生产过程中遇到上述问题通常采用流水泥浆、聚氨酯类、环氧类等材料对巷道工作面顶板进行维护,但是上述材料在实际应用中给安全生产带来诸多的问题。如下所述:
1.煤矿地质裂隙微细,水泥注浆粒径大,扩散半径小,微小裂隙注不进,固化时间不可调; 
2.煤矿井下环境潮湿有水,聚氨酯类遇水发泡,强度降低;
3.有机类(聚氨酯、环氧类)的注浆材料反应热高、阻燃性低,容易引起煤矿火灾 。
发明内容
本发明所要解决的技术问题是提供一种矿用水玻璃加固堵水材料,目的是以达到矿用加固材料阻燃性高、反应热低、固化时间可调、环境水对反应基本无影响的效果,很大程度上提高了煤矿的生产的安全性。
本发明的技术方案:一种矿用水玻璃加固堵水材料,由两种独立的A组份与B组份组成,A组份和B组份按照体积比为1~2:1的比例混合,其中所述A组份的原料按照重量百分数为:水玻璃A:51~99.9%,水玻璃B:0~50%,催化剂C:0.1~2%, 增塑剂D:0~50% ;其中所述B组份的原料按照重量百分数为:固化剂A:51~100% , 固化剂B:0~50%,聚醚多元醇C:0~50% 。
所述的水玻璃A为模数为1.5~3.5的钠水玻璃、钾水玻璃、钠钾水玻璃中的一种或一种以上。
所述的水玻璃B为模数为1.5~3.5的钠水玻璃、钾水玻璃、钠钾水玻璃中的一种或一种以上。
所述的催化剂C为N、N-二甲基苄胺、三聚催化剂2,4,6-三(二甲氨基甲基)苯酚、二甲基环已胺、五甲基二亚乙基三胺、二甲基乙醇胺、2,2-双吗啉基二乙基醚、二月桂酸二丁基锡、二醋酸二丁基锡、钛酸四丁酯中的一种或一种以上。
所述的增塑剂D为邻苯二甲酸二辛酯、邻苯二甲酸二丁脂、甘油三醋酸酯、柠檬酸三乙酯、乙酰柠檬酸三乙酯、柠檬酸三丁酯、乙酰柠檬酸三(2-乙基已)酯、氯化石蜡中的一种或一种以上。
所述的固化剂A为多苯基多亚甲基多异氰酸酯。
所述的固化剂B为1,4丁内酯、十二烷基苯磺酸钠、乙二醇、碳酸丙烯酯、甘油三醋酸酯、乙二醇乙醚醋酸酯中的一种或一种以上。
所述的聚醚多元醇C为2官能度,分子量为500~3000聚氧化丙烯二醇和聚四氢呋喃二醇中的一种或一种以上。
一种矿用水玻璃加固堵水材料的制备方法,包括以下步骤:
a.制备A组份料:先将51~99.9%的水玻璃A与0~50%的水玻璃B装入反应釜中,然后依次加入0.1~2%的催化剂C和0~50%的增塑剂D,在常温下搅拌均匀,待所有组份反应稳定取样检测合格后,即密封包装;
b.制备B组份料:先将51~100%的固化剂A装入反应釜中,然后加入0~50%的聚醚多元醇C,在30~45℃下搅拌均匀后再加入0~50%的固化剂B,取样检测合格后,即可密封包装;
     使用时用高压注浆泵将制备好的A组份与B组份按照1~2:1的体积比混合注入煤岩体中,材料将会渗透到微小裂隙,发生膨胀固化反应,达到加固稳固支撑煤岩体的目的。所述的高压注浆泵为双液压注浆泵。
本发明制得的矿用水玻璃加固堵水材料产品质量指标如下:
(1)固化时间60s~300s;
(2)发泡倍率≧1倍;
(3)抗压强度≧35 MPa;
(4)阻燃性:不燃。 
本发明的有益效果:
1. 本发明矿用水玻璃加固堵水材料粘度小、流动性好、渗透性强、固化时间可调、高阻燃、低反应热、环境水对反应基本无影响、固结物强度高,能为煤矿安全生产和高效生产提供保障;
2. 本发明矿用水玻璃加固堵水材料价格低廉、施工方便、安全阻燃、综合性能高,完全满足煤矿企业的需求,符合绿色化和可持续发展要求;
3. 本发明矿用水玻璃加固堵水材料还可以用于建筑地基加固,交通路基加固、隧道加固等行业。
具体实施方式
以下结合实施例对本发明作进一步说明
实施例1
一种矿用水玻璃加固堵水材料, 按以下重量比原料配制而成:
A组份料:分别称量水玻璃A模数为1.5的钠水玻璃51千克,水玻璃B模数为1.5的钠钾水玻璃34千克,催化剂C五甲基二亚乙基三胺0.15千克、三聚催化剂2,4,6-三(二甲氨基甲基)苯酚0.25千克和二月桂酸二丁基锡0.1千克,增塑剂D 52#氯化石蜡14.5千克。将称量好的水玻璃A、水玻璃B装入混合釜中搅拌,然后分别加入称量好的催化剂C和增塑剂D,在常温下搅拌均匀,取样检测合格后,即可密封包装。
B组份料:分别称量固化剂A多苯基多亚甲基多异氰酸酯(烟台万华PM-200)51千克 ,固化剂B甘油三醋酸酯26千克,聚醚多元醇C为2官能度分子量为500的聚氧化丙烯二醇23千克。将称量好的固化剂A、聚醚多元醇C装入混合釜,在30℃搅拌均匀反应后,然后加入称量好的固化剂B,搅拌均匀,取样检测合格后,即可密封包装。
将A组份与B组份经高压气动注浆泵按照体积比1:1在静态混合器混合合得到固结体,检测产品质量指标:固化时间160s,发泡倍率1.3倍,抗压强度40.9MPa,阻燃性:不燃,符合煤矿使用标准。
实施例2
一种矿用水玻璃加固堵水材料, 按以下重量比原料配制而成:
A组份料:分别称量水玻璃A模数为2.6的钠水玻璃70千克,水玻璃B模数为2的钠钾水玻璃15千克,催化剂C五甲基二亚乙基三胺0.2千克、二甲基乙醇胺0.3千克、二甲基环已胺0.5千克,增塑剂D为52#氯化石蜡10千克和邻苯二甲酸二丁脂4千克。将称量好的水玻璃A、水玻璃B装入混合釜中搅拌,然后分别加入称量好的催化剂C和增塑剂D,在常温下搅拌均匀,取样检测合格后,即可密封包装。
B组份料:分别称量固化剂A烟台万华PM-200多苯基多亚甲基多异氰酸酯70千克 ,固化剂B甘油三醋酸酯15千克,聚醚多元醇C为2官能度分子量为1000的聚氧化丙烯二醇15千克。将称量好的固化剂A、聚醚多元醇C装入混合釜,在35℃搅拌均匀反应后,然后加入称量好的固化剂B,搅拌均匀,取样检测合格后,即可密封包装。
将A组份与B组份经高压气动注浆泵按照体积比1.2:1在静态混合器混合合得到固结体,检测产品质量指标:固化时间90s,发泡倍率1.4倍,抗压强度42.7MPa,阻燃性:不燃,符合煤矿使用标准。
实施例3
一种矿用水玻璃加固堵水材料, 按以下重量比原料配制而成:
A组份料:分别称量水玻璃A模数为3的钠水玻璃80千克,水玻璃B模数为2.5的钠水玻璃10千克,催化剂C为N、N-二甲基苄胺0.25千克、三聚催化剂2,4,6-三(二甲氨基甲基)苯酚0.15千克和二月桂酸二丁基锡0.1千克,增塑剂D为52#氯化石蜡5千克和邻苯二甲酸二丁脂4.5千克。将称量好的水玻璃A、水玻璃B装入混合釜中搅拌,然后分别加入称量好的催化剂C和增塑剂D,在常温下搅拌均匀,取样检测合格后,即可密封包装。
B组份料:分别称量固化剂A烟台万华PM-200多苯基多亚甲基多异氰酸酯85千克 ,固化剂B甘油三醋酸酯3千克,聚醚多元醇C为2官能度分子量为2000的聚氧化丙烯二醇12千克。将称量好的固化剂A、聚醚多元醇C装入混合釜,在40℃搅拌均匀反应后,然后加入称量好的固化剂B,搅拌均匀,取样检测合格后,即可密封包装。
将A组份与B组份经高压气动注浆泵按照体积比1.4:1在静态混合器混合得到固结体,检测产品质量指标:固化时间150s,发泡倍率1.2倍,抗压强度41.7MPa,阻燃性:不燃,符合煤矿使用标准。
实施例4
一种矿用水玻璃加固堵水材料, 按以下重量比原料配制而成:
A组份料:分别称量水玻璃A模数为3.5的钠水玻璃99.9千克,水玻璃B模数为3.5的钠钾水玻璃0千克,催化剂C为二甲基环已胺0.1千克,增塑剂D为52#氯化石蜡0千克。将称量好的水玻璃A、水玻璃B装入混合釜中搅拌,然后分别加入称量好的催化剂C和增塑剂D,在常温下搅拌均匀,取样检测合格后,即可密封包装。
B组份料:分别称量固化剂A烟台万华PM-200多苯基多亚甲基多异氰酸酯100千克 ,固化剂B乙二醇乙醚醋酸酯0千克,聚醚多元醇C为2官能度分子量为3000的聚四氢呋喃二醇0千克。将称量好的固化剂A、聚醚多元醇C装入混合釜,在45℃搅拌均匀反应后,然后加入称量好的固化剂B,搅拌均匀,取样检测合格后,即可密封包装。
将A组份与B组份经高压气动注浆泵按照体积比2:1在静态混合器混合合得到固结体,检测产品质量指标:固化时间90s,发泡倍率1.45倍,抗压强度43.6MPa,阻燃性:不燃,符合煤矿使用标准。

Claims (8)

1.一种矿用水玻璃加固堵水材料,其特征是由两种独立的A组份与B组份组成, A组份和B组份按照体积比为1~2:1的比例混合,其中所述A组份的原料按照重量百分数为:水玻璃A:51~99.9%,水玻璃B:0~50%,催化剂C:0.1~2%, 增塑剂D:0~50% ;其中所述B组份的原料按照重量百分数为:固化剂A:51~100% , 固化剂B:0~50%,聚醚多元醇C:0~50% 。
2.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的水玻璃A为模数为1.5~3.5的钠水玻璃、钾水玻璃、钠钾水玻璃中的一种或一种以上。
3.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的水玻璃B为模数为1.5~3.5的钠水玻璃、钾水玻璃、钠钾水玻璃中的一种或一种以上。
4.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的催化剂C为N、N-二甲基苄胺、三聚催化剂2,4,6-三(二甲氨基甲基)苯酚、二甲基环已胺、五甲基二亚乙基三胺、二甲基乙醇胺、2,2-双吗啉基二乙基醚、二月桂酸二丁基锡、二醋酸二丁基锡、钛酸四丁酯中的一种或一种以上。
5.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的增塑剂D为邻苯二甲酸二辛酯、邻苯二甲酸二丁脂、甘油三醋酸酯、柠檬酸三乙酯、乙酰柠檬酸三乙酯、柠檬酸三丁酯、乙酰柠檬酸三(2-乙基已)酯、氯化石蜡中的一种或一种以上。
6.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的固化剂A为多苯基多亚甲基多异氰酸酯。
7.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的固化剂B为1,4丁内酯、十二烷基苯磺酸钠、乙二醇、碳酸丙烯酯、甘油三醋酸酯、乙二醇乙醚醋酸酯中的一种或一种以上。
8.根据权利要求1所述的一种矿用水玻璃加固堵水材料,其特征是所述的聚醚多元醇C为2官能度,分子量为500~3000聚氧化丙烯二醇和聚四氢呋喃二醇中的一种或一种以上。
CN2013100477868A 2013-02-06 2013-02-06 一种矿用水玻璃加固堵水材料 Pending CN103113079A (zh)