CN102863898B - Cracking resistance texture coating preparation method and goods thereof - Google Patents

Cracking resistance texture coating preparation method and goods thereof Download PDF

Info

Publication number
CN102863898B
CN102863898B CN201210344490.8A CN201210344490A CN102863898B CN 102863898 B CN102863898 B CN 102863898B CN 201210344490 A CN201210344490 A CN 201210344490A CN 102863898 B CN102863898 B CN 102863898B
Authority
CN
China
Prior art keywords
water
cracking resistance
easy
thickener
mixture
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201210344490.8A
Other languages
Chinese (zh)
Other versions
CN102863898A (en
Inventor
张立功
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Huang Mingjie
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201210344490.8A priority Critical patent/CN102863898B/en
Publication of CN102863898A publication Critical patent/CN102863898A/en
Application granted granted Critical
Publication of CN102863898B publication Critical patent/CN102863898B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of cracking resistance texture coating preparation method, also disclose a kind of goods that the method makes of implementing; The raw material components of these goods comprises water, ethylene glycol, cellulose, anticorrisive agent, PH conditioning agent, dicalcium powder, defoamer, elastic emulsion, TEXANOL and thickener; The preparation technology of method provided by the invention is simple and easy, be easy to realize, and production efficiency is high; The preparation technology of method provided by the invention is simple and easy, be easy to realize, and production efficiency is high; The formula Design of cracking resistance texture coating goods provided by the invention is reasonable, and hot strength is good, and cracking resistance is water-fast, strong adhesion, can better be bonded on body of wall, and weather-proof decorative effect is excellent, ensure that body of wall outward appearance is clean and tidy, elegant in appearance, match volume is good, and good combination property, there is good temperature tolerance and weatherability, not easy to crack, long service life, effectively reduces maintenance cost, and working procedure is simple and easy in addition, reduction of erection time greatly, improve efficiency of construction and with low cost, be beneficial to wide popularization and application.

Description

Cracking resistance texture coating preparation method and goods thereof
Technical field
The invention belongs to paint technical field, be specifically related to a kind of cracking resistance texture coating preparation method and implement the method makeGoods.
Background technology
Texture coating is exactly to be coated with the coating material sense of reality of spreading after wall to be called texture. The inspiration of texture coating the earliest fromThe cabin of the different style on the Greece peninsula, is widely used in a large number in foreign country, and domestic manufacturer passed through technology in recent yearsIntroduce texture coating is taken to domestic construction industry, create much of a stir immediately, its lines, honesty, thick and heavy sensation, allows people enjoyStyle under the landscape of the peninsula, domestic manufacturers are after introduction, and the improvement of having carried out formula makes it to adapt to high weather-proof and Chinese marketFeature.
Texture coating, with the individual character collocation of its with countless changes three-dimensional texture, more options, represents unique visual angle, space,Abundant and lively, make us fresh and new. And create to meet Integral decoration style with individual character, make texture coating in decorationShow the individual style of oneself. This Novel artistic coating has been brought natural environmental-protective type in the smooth type epoch of wall body coatingThe brand-new epoch of concavo-convex coating. Can substitute wallpaper, and environmental protection more, economy, personalization. Texture coating is radiationless, deadweightGently, effect is true to nature, and by different construction technologies, gimmick and skill, create infinite special decorative effect. On Here it is market justAt popular novel decorative new material--texture coating. Be widely used at present villa, hotel, office, rural windThe building of lattice, high class residential zone, is also widely used in indoor pastoralism finishing etc. by people.
Texture coating is exactly mainly to use special instrument to mould on the wall different moulding and pattern, makes space moreSolid and truly elegant in appearance. The current domestic whole texture coating market of making a general survey of, although it can meet common instructions for use,But its hot strength is low, and adhesive force is general, be prone to cracking or peeling phenomenon, cause rainwater just to infiltrate metope, corrosion metope,Affect outward appearance, greatly reduce decorative effect.
Therefore researching and developing the cracking resistance texture coating that a kind of cracking resistance, adhesive force and closure are good is work as generation required.
Summary of the invention
For above-mentioned deficiency, one of the object of the invention is, provides a kind of manufacturing process simple and easy, is easy to realize, and producesThe cracking resistance texture coating preparation method that efficiency is high;
Two of the object of the invention is, a kind of goods of implementing above-mentioned cracking resistance texture coating preparation method are provided. These goodsCracking resistance, adhesive force and closure are good.
For achieving the above object, technical scheme provided by the present invention is:
A kind of cracking resistance texture coating preparation method, is characterized in that, it comprises the following steps:
(1) preparing material, each component and the percentage by weight thereof of raw material are as follows:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
Hydroxyethylcellulose 0.2-0.3%,
Anticorrisive agent 0.2-0.4%,
PH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
Elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
Thickener 0.3-0.5%,
Second part of water 0.3-0.5%;
(2) first part of water and ethylene glycol are dropped into a mixing bowl, start a mixing bowl and stir action, then slowly add hydroxylEthyl cellulose, is stirred to hydroxyethylcellulose and dissolves completely, makes the first mixture;
(3) by anticorrisive agent, PH conditioning agent, dicalcium powder, defoamer and and elastic emulsion add in the first mixture, wait to stirEvenly, make the second mixture;
(4) TEXANOL is slowly added in the second mixture, after stirring, make the 3rd mixture;
(5) take thickener and second part of water of corresponding proportional quantity according to required working viscosity, then by thickener andSecond part of water mixes, and then adds the 3rd mixture, and stirs, and makes cracking resistance texture coating.
Described hydroxyethylcellulose is ER-30M hydroxyethylcellulose,
Described anticorrisive agent is LXE anticorrisive agent, and described conditioning agent is AMP-95PH conditioning agent, and described elastic emulsion is BLJ-938 elastic emulsions.
Described thickener is ASE-60 thickener.
The speed setting of a mixing bowl in described step (2) is that 300-500 Zhuan ∕ divides, and mixing time is 15-30 minute.
Implement the goods that above-mentioned cracking resistance texture coating preparation method makes, its each component and weight percent thereof such asUnder:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
Hydroxyethylcellulose 0.2-0.3%,
Anticorrisive agent 0.2-0.4%,
PH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
Elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
Thickener 0.3-0.5%,
Second part of water 0.3-0.5%.
Described hydroxyethylcellulose is ER-30M hydroxyethylcellulose.
Described anticorrisive agent is LXE anticorrisive agent, and described conditioning agent is AMP-95PH conditioning agent.
Described elastic emulsion is BLJ-938 elastic emulsion.
Described thickener is ASE-60 thickener.
Beneficial effect of the present invention is: the preparation technology of method provided by the invention is simple and easy, be easy to realize production efficiencyHigh; The formula Design of cracking resistance texture coating goods provided by the invention is reasonable, and hot strength is good, and cracking resistance is water-fast, strong adhesion,Can better be bonded on body of wall, bonding is firm, the test that can bear rainforest, high temperature, and weather-proof decorative effect is excellent, ensures body of wall outward appearanceNeatly, elegant in appearance, match volume is good, and good combination property, has good temperature tolerance and weatherability, not easy to crack, makesLong with the life-span, effectively reduce maintenance cost, in addition, working procedure is simple and easy, the reduction of erection time greatly, improves efficiency of construction and cost lowHonest and clean, be beneficial to wide popularization and application.
Below in conjunction with embodiment, the invention will be further described.
Detailed description of the invention
Embodiment 1: a kind of cracking resistance texture coating preparation method that the present embodiment provides, it is characterized in that, it comprises followingStep:
(1) preparing material, each component and the percentage by weight thereof of raw material are as follows:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
Hydroxyethylcellulose 0.2-0.3%,
Anticorrisive agent 0.2-0.4%,
PH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
Elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
Thickener 0.3-0.5%,
Second part of water 0.3-0.5%;
(2) first part of water and ethylene glycol are dropped into a mixing bowl, start a mixing bowl and stir action, then slowly add hydroxylEthyl cellulose, is stirred to hydroxyethylcellulose and dissolves completely, makes the first mixture;
(3) by anticorrisive agent, PH conditioning agent, dicalcium powder, defoamer and and elastic emulsion add in the first mixture, wait to stirEvenly, make the second mixture;
(4) TEXANOL is slowly added in the second mixture, after stirring, make the 3rd mixture;
(5) take thickener and second part of water of corresponding proportional quantity according to required working viscosity, then by thickener andSecond part of water mixes, and then adds the 3rd mixture, and stirs, and makes cracking resistance texture coating.
Described hydroxyethylcellulose is ER-30M hydroxyethylcellulose,
Described anticorrisive agent is LXE anticorrisive agent, and described conditioning agent is AMP-95PH conditioning agent, and described elastic emulsion is BLJ-938 elastic emulsions.
Described thickener is ASE-60 thickener.
The speed setting of a mixing bowl in described step (2) is that 300-500 Zhuan ∕ divides, and mixing time is 15-30 minute.
Implement the goods that above-mentioned cracking resistance texture coating preparation method makes, its each component and weight percent thereof such asUnder:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
Hydroxyethylcellulose 0.2-0.3%,
Anticorrisive agent 0.2-0.4%,
PH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
Elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
Thickener 0.3-0.5%,
Second part of water 0.3-0.5%.
Described hydroxyethylcellulose is ER-30M hydroxyethylcellulose.
Described anticorrisive agent is LXE anticorrisive agent, and described conditioning agent is AMP-95PH conditioning agent.
Described elastic emulsion is BLJ-938 elastic emulsion.
Described thickener is ASE-60 thickener.
In the present embodiment, described ethylene glycol and ER-30M hydroxyethylcellulose can be buied in Tao Shi producer;
In the present embodiment, described LXE anticorrisive agent and ASE-60 thickener can be buied in ROHM AND HAAS producer;
In the present embodiment, described NXZ defoamer can be buied in Nuo Puke producer;
In the present embodiment, described BLJ-938 elastic emulsion can be buied in Bao Lijia producer;
In the present embodiment, described dicalcium powder can be buied in Long Guang talcum producer;
In the present embodiment, described TEXANOL can buy in Yi Shiman producer;
In the present embodiment, described Snow Flower White can be buied in He Prefecture Wei Ying flour sand producer;
In the present embodiment, preferably 300 order dicalcium powders.
In other embodiment, can choose from other manufacturer or supplier, and select other to there is similarityModel or the article of type substitute.
Embodiment 2: the goods that a kind of above-mentioned cracking resistance texture coating preparation method makes, its each component and weight percent thereofThan as follows:
First part of water 8%,
Ethylene glycol 0.5%,
Hydroxyethylcellulose 0.2%,
Anticorrisive agent 0.2%,
PH conditioning agent 0.2%,
200-400 order dicalcium powder 12%,
Defoamer 0.3%,
Elastic emulsion 25%,
TEXANOL3%,
30-60 order Snow Flower White 50%,
Thickener 0.3%,
Second part of water 0.3%.
Embodiment 3: its from the difference of embodiment 2 be component in goods with and percentage by weight different. Its each groupPoint and percentage by weight as follows:
First part of water 12%,
Ethylene glycol 1%,
Hydroxyethylcellulose 0.3%,
Anticorrisive agent 0.4%,
PH conditioning agent 0.1%,
200-400 order dicalcium powder 9%,
Defoamer 0.2%,
Elastic emulsion 19%,
TEXANOL6%,
30-60 order Snow Flower White 51%,
Thickener 0.5%,
Second part of water 0.5%.
Embodiment 4: its from the difference of embodiment 2 be component in goods with and percentage by weight different. Its each groupPoint and percentage by weight as follows:
First part of water 8.35%,
Ethylene glycol 0.55%,
Hydroxyethylcellulose 0.25%,
Anticorrisive agent 0.25%,
PH conditioning agent 0.15%,
200-400 order dicalcium powder 8%,
Defoamer 0.25%,
Elastic emulsion 18%,
TEXANOL3.5%,
30-60 order Snow Flower White 60%,
Thickener 0.35%,
Second part of water 0.35%.
The preparation technology of method provided by the invention is simple and easy, be easy to realize, and production efficiency is high.
The formula Design of cracking resistance texture coating goods provided by the invention is reasonable, and hot strength is good, and cracking resistance is water-fast, adheres toPower is strong, can better be bonded on body of wall, and bonding is firm, the test that can bear rainforest, high temperature, and weather-proof decorative effect is excellent, ensures wallExternal sight is clean and tidy, elegant in appearance, and match volume is good, and good combination property, has good temperature tolerance and weatherability, is difficult for outSplit, long service life, effectively reduces maintenance cost, and in addition, working procedure is simple and easy, the reduction of erection time greatly, improve efficiency of construction andWith low cost, be beneficial to wide popularization and application.
Above-described embodiment is only the good embodiment of the present invention, and the present invention can not enumerate out whole enforcement sidesFormula, the technical scheme of one of all employing above-described embodiments, or the equivalent variations of doing according to above-described embodiment, all protect in the present inventionProtect in scope.
As described in the above embodiment the present invention, adopt method same or similar with it and component and other cracking resistance matter of obtainingSense preparation method for coating and goods, all in protection domain of the present invention.

Claims (2)

1. a cracking resistance texture coating preparation method, is characterized in that, it comprises the following steps:
(1) preparing material, each component and the percentage by weight thereof of raw material are as follows:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
ER-30M hydroxyethylcellulose 0.2-0.3%,
LXE anticorrisive agent 0.2-0.4%,
AMP-95pH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
BLJ-938 elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
ASE-60 thickener 0.3-0.5%,
Second part of water 0.3-0.5%;
(2) first part of water and ethylene glycol are dropped into a mixing bowl, start a mixing bowl and stir action, the speed setting of a mixing bowl is300-500 Zhuan ∕ divides, and mixing time is 15-30 minute; Then slowly add ER-30M hydroxyethylcellulose, be stirred to ER-30M hydroxyethylcellulose dissolves, and makes the first mixture;
(3) anticorrisive agent, pH adjusting agent, dicalcium powder, defoamer and elastic emulsion are added in the first mixture, wait to stirAfter, make the second mixture;
(4) TEXANOL is slowly added in the second mixture, after stirring, make the 3rd mixture;
(5) take thickener and second part of water of corresponding proportional quantity according to required working viscosity, then by thickener and secondPart water mixes, and then adds the 3rd mixture, and stirs, and makes cracking resistance texture coating.
2. implement the claims the goods that described in 1, cracking resistance texture coating preparation method makes, it is characterized in that, its each groupPoint and percentage by weight as follows:
First part of water 8-12%,
Ethylene glycol 0.5-1%,
ER-30M hydroxyethylcellulose 0.2-0.3%,
LXE anticorrisive agent 0.2-0.4%,
AMP-95pH conditioning agent 0.1-0.2%,
200-400 order dicalcium powder 8-12%,
Defoamer 0.2-0.3%,
BLJ-938 elastic emulsion 18-25%,
TEXANOL3-6%,
30-60 order Snow Flower White 50-60%,
ASE-60 thickener 0.3-0.5%,
Second part of water 0.3-0.5%.
CN201210344490.8A 2012-09-18 2012-09-18 Cracking resistance texture coating preparation method and goods thereof Expired - Fee Related CN102863898B (en)