CN102809561B - 一种快速确定aod还原效果的方法 - Google Patents

一种快速确定aod还原效果的方法 Download PDF

Info

Publication number
CN102809561B
CN102809561B CN201210294065.2A CN201210294065A CN102809561B CN 102809561 B CN102809561 B CN 102809561B CN 201210294065 A CN201210294065 A CN 201210294065A CN 102809561 B CN102809561 B CN 102809561B
Authority
CN
China
Prior art keywords
basicity
mass percentage
percentage content
aod
blast furnace
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210294065.2A
Other languages
English (en)
Other versions
CN102809561A (zh
Inventor
翟俊
刘亮
刘卫东
马骏鹏
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanxi Taigang Stainless Steel Co Ltd
Original Assignee
Shanxi Taigang Stainless Steel Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanxi Taigang Stainless Steel Co Ltd filed Critical Shanxi Taigang Stainless Steel Co Ltd
Priority to CN201210294065.2A priority Critical patent/CN102809561B/zh
Publication of CN102809561A publication Critical patent/CN102809561A/zh
Application granted granted Critical
Publication of CN102809561B publication Critical patent/CN102809561B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种快速确定AOD还原效果的方法,属于炼钢领域,它包括通过采集大量数据制成的典型AOD还原炉渣的比色卡,所述比色卡是采集碱度1.74~2.00,Cr2O3质量百分比含量0.23%~0.78%范围内的还原炉渣比色卡,通过将还原炉渣的颜色与比色卡的颜色进行比较,来确定还原炉渣的碱度和Cr2O3质量百分比含量,从而判定AOD还原效果。本发明使AOD炉渣碱度和Cr2O3的分析时间由2~4h缩短到5~10min。

Description

一种快速确定AOD还原效果的方法
技术领域
本发明属于炼钢领域,具体涉及一种快速确定AOD还原效果的方法。
背景技术
AOD还原效果直接影响不锈钢钢水的洁净度,钢水洁净度不仅会影响连铸坯冷轧后的表面冷板质量,还会影响连铸过程保护渣的性能,间接影响连铸坯表面质量。
连铸坯表面质量的好坏对冷轧板表面质量有直接的影响,如若控制不好,影响钢种成材率、增加生产成本,降低公司产品竞争力。
目前判断AOD还原效果的方法主要有两种,第一种:通过判断一次还原S的高低,间接判断还原效果。该方法精度不够高;第二种:分析还原炉渣成分,通过炉渣的碱度和Cr2O3的高低来确定钢水还原效果。
AOD还原炉渣分析成分时间长,目前最快的分析速度也需要2~4h。由于分析时间较长,不能快速、有效判断钢水洁净度是否对连铸过程有影响,对大生产没有太大的指导意义。另外,如果想确定还原效果,必须每炉钢都需要分析炉渣成分,增加劳动成本,降低生产效率。
所以如何能及时、准确判断AOD还原效果对目前AOD生产不锈钢有很重要的意义。
发明内容
本发明提供一种在十分钟之内快速确定AOD还原效果的方法。
本发明是将还原炉渣的颜色与比色卡的颜色进行对比,快速确定渣中Cr2O3含量和炉渣碱度,从而快速确定钢水的还原效果。
本发明包括通过采集大量典型炉渣的碱度和Cr2O3百分比含量的颜色数据,颜色数据碱度的范围为1.74~2.00,Cr2O3质量百分比含量为0.23%~0.78%,制成典型炉渣成分图片卡作为比色卡。
本发明包括下述十种典型炉渣的比色卡。
碱度是2.0,Cr2O3质量百分比含量是0.23%;
碱度是1.74,Cr2O3质量百分比含量是0.53%;
碱度是1.84,Cr2O3质量百分比含量是0.36%;
碱度是1.95,Cr2O3质量百分比含量是0.56%;
碱度是1.80,Cr2O3质量百分比含量是0.62%;
碱度是1.93,Cr2O3质量百分比含量是0.62%;
碱度是1.89,Cr2O3质量百分比含量是0.37%;
碱度是1.75,Cr2O3质量百分比含量是0.76%;
碱度是1.92,Cr2O3质量百分比含量是0.4%;
碱度是1.82,Cr2O3质量百分比含量是0.78%。
通过还原炉渣碱度与Cr2O3质量百分比含量确定AOD还原效果好的指标是碱度为1.85~1.95,Cr2O3质量百分比含量为0.2~0.4%。
本发明炉渣炉渣碱度和Cr2O3含量涵盖了目前大生产AOD冶炼不锈钢还原炉渣的范围,使用精确达到95%以上。
本发明可以在5~10min之内快速确定AOD还原效果。它有效解决了炼钢生产现场不能及时确定AOD还原效果的矛盾,对指导大生产具有非常重要的意义。
使用AOD炉渣还原比色卡,快速确定还原效果的步骤如下:
取还原渣样
AOD还原结束后,用钢棒插入AOD炉渣里面,蘸取还原炉渣。将钢棒表面蘸取的还原炉渣放到干净的白纸上面。
与比色卡上的颜色对比
   肉眼观察还原炉渣颜色与比色卡上的颜色,确定还原炉渣颜色与比色卡的哪张相近,就可以确定炉渣的碱度和Cr2O3含量。
确定对比结果
   通过对比,确定炉渣还原效果,确定AOD下一步操作。
具体实施方式
实施例1
11:23 AOD还原结束,硬用钢棒蘸取还原渣样;
11:25 AOD还原渣样放到干净的白纸上面,通过肉眼与比色卡对比;
11:27确定对比结果:碱度 1.92,Cr2O0.40%。
说明本实施例还原效果好
实施例2
14:36 AOD还原结束,硬用钢棒蘸取还原渣样;
14:41 AOD还原渣样放到干净的纸张上面,通过肉眼与比色卡对比;
14:43确定对比结果:碱度 1.75,Cr2O0.76%。
说明本实施例还原效果差,碱度低,Cr2O3含量高。
实施例3
08:06 AOD还原结束,硬用钢棒蘸取还原渣样;
08:12 AOD还原渣样放到干净的纸张上面,通过肉眼与比色卡对比;
08:15确定对比结果:碱度 1.95,Cr2O0.56%。
说明本实施例还原效果一般,碱度合适,但是Cr2O3含量高。

Claims (1)

1.一种快速确定AOD还原效果的方法,包括下述十种典型炉渣的比色卡:
碱度是2.0,Cr2O3质量百分比含量是0.23%;
碱度是1.74,Cr2O3质量百分比含量是0.53%;
碱度是1.84,Cr2O3质量百分比含量是0.36%;
碱度是1.95,Cr2O3质量百分比含量是0.56%;
碱度是1.80,Cr2O3质量百分比含量是0.62%;
碱度是1.93,Cr2O3质量百分比含量是0.62%;
碱度是1.89,Cr2O3质量百分比含量是0.37%;
碱度是1.75,Cr2O3质量百分比含量是0.76%;
碱度是1.92,Cr2O3质量百分比含量是0.4%;
碱度是1.82,Cr2O3质量百分比含量是0.78%;
具体操作步骤如下:
(1)、取还原渣样,即AOD还原结束后,用钢棒插入AOD炉渣里面,蘸取还原炉渣,将钢棒表面蘸取的还原炉渣放到干净的白纸上面;
2)、与比色卡上的颜色对比,即用肉眼观察还原炉渣颜色与比色卡上的颜色,确定还原炉渣颜色与比色卡的哪张相近,就可以确定炉渣的碱度和Cr2O3含量;
3)、确定对比结果,当炉渣碱度为1.85~1.95,Cr2O3质量百分比含量为0.2~0.4%,判定AOD还原效果好。
CN201210294065.2A 2012-08-17 2012-08-17 一种快速确定aod还原效果的方法 Active CN102809561B (zh)