CN102505348A - 超柔sms非织造布的制备方法 - Google Patents

超柔sms非织造布的制备方法 Download PDF

Info

Publication number
CN102505348A
CN102505348A CN2011103842493A CN201110384249A CN102505348A CN 102505348 A CN102505348 A CN 102505348A CN 2011103842493 A CN2011103842493 A CN 2011103842493A CN 201110384249 A CN201110384249 A CN 201110384249A CN 102505348 A CN102505348 A CN 102505348A
Authority
CN
China
Prior art keywords
spunbond
sms
fibre
melt
fibre web
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2011103842493A
Other languages
English (en)
Inventor
陈建国
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHEJIANG SANXIANG NEW MATERIAL TECHNOLOGY Co Ltd
Original Assignee
ZHEJIANG SANXIANG NEW MATERIAL TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHEJIANG SANXIANG NEW MATERIAL TECHNOLOGY Co Ltd filed Critical ZHEJIANG SANXIANG NEW MATERIAL TECHNOLOGY Co Ltd
Priority to CN2011103842493A priority Critical patent/CN102505348A/zh
Publication of CN102505348A publication Critical patent/CN102505348A/zh
Pending legal-status Critical Current

Abstract

超柔SMS非织造布的制备方法,SMS原料包括以下重量比的材料:PP纺粘树脂40-70%、熔喷树脂15-30%、PP/PE共聚体的改性树脂10-30%、色母粒2-5%。制备方法,包括以下步骤:a.熔体准备与纺丝、b.牵伸、c.成网、d.热轧加固、e.卷绕。通过在SMS生产线上的多次试验与论证,依据本发明制备的SMS非织造布柔软度测试均优于常规产品。

Description

超柔SMS非织造布的制备方法
技术领域:
本发明涉及一种超柔SMS非织造布的制备方法。
技术背景
随着市场经济的发展,用户对产品质量要求越来越高。
由于SMS非织造布产品具有强力高、生产成本低、耐磨性好、过滤效率高、阻隔性能强的特点,已在医疗、卫生、保健领域得到了广泛的应用,而经过抗静电、拒水、拒酒精、拒血液功能处理的产品更是高端医疗防护用品的首选材料。
自婴幼儿用纸尿裤的背层、防侧漏材料有短纤热粘合非织造布改为SMS材料后,全球SMS非织造布出现了短暂的紧张;除了卫生用品外,该类产品已向医疗用品市场进军,从全球看,目前在手术包布、手术衣、手术洞巾方面SMS产品已占主导地位;
随着手术服性能要求的提高、SMS产品的优点更为突出,许多原先用水刺无纺布的产品逐步转而采用SMS材料;
但是常规SMS产品由于采用的是热轧的方式制备的,导致手感较硬,和水刺布相比还有距离,这一点使得SMS产品的应用得到一定的限制,特别是欧美一些对手术服综合性能要求比较高的国家,解决SMS产品手感及舒适问题是摆在SMS产品的一个重要课题,包括着衣的声响、柔软性、皮肤刺激、透气性、防静电及重量等,另外兼顾防护性包括抗血液、抗酒精等等;
通过改善SMS产品的纤维性能和产品组分结构,使产品手感变软,是一个十分必要和有意义的课题,多组份的超柔SMS非织造布就是根据市场的发展与需求而衍生的新产品。
发明内容
为了解决上述问题,达到上述目的,本发明要解决的技术问题在于提供一种多组份的超柔SMS非织造布制备方法工艺。使用该工艺方法可以极大的提高产品的手感与柔软度。
常规工艺流程简图如下:附图1为常规纺粘(简写S)流程简图、附图2为常规熔喷(简写M)流程简图、附图3为常规SMS生产工艺流程简图,但是常规工艺流程制备的SMS产品柔软度不够理想。
本发明采用如下技术方案:超柔SMS非织造布制备方法,依次包括熔体准备与纺丝(原料计量混合、上料、挤压熔融、熔体过滤、纺丝)、牵伸、成网、热扎加固、卷绕这几个步骤,关键在于原料的选择与计量混合。PP树脂在一定的加工工艺中,相对而言比PE偏挺与硬,基于该特性就选择在PP纺粘树脂和熔喷树脂中加入10-30%(较好的是20-30%)的PP/PE改性树脂,在PP/PE改性树脂的选择中对其的物性的分析与添加比例是关键,既需要符合纺丝,又需要该改性树脂满足与PP聚丙烯相容的要求,与纺粘树脂计量混合进入纺丝,经过牵伸成网定型。具体技术方案是:
SMS原料包括以下重量比的材料:
PP纺粘树脂比例40-70%、熔喷树脂比例15-30%、PP/PE共聚体的改性树脂比例10-30%、色母粒比例2-5%。
超柔SMS非织造布的制备方法包括以下步骤:
a.熔体准备与纺丝
聚丙烯树脂和熔喷用高熔融指数聚丙烯树脂以及添加相关的PP/PE共聚体的改性树脂通过自动输送系统输送到各自的储存料斗,与相关的添加剂按一定比例自动计量混和后进入螺杆挤压机,经挤压、熔融、计量,以一定的温度、压力进入熔体过滤器,除去杂质后,再经静态混和器进一步混和均匀,再经纺丝计量泵计量,进入纺丝组件过滤、混和、均匀后,由喷丝板喷出。
b.牵伸
纺粘冷却后的丝束被导入牵伸器,在牵伸器中心部延宽度方向有一牵伸槽,两侧吹入高压空气,丝束在牵伸槽中经高压空气牵伸后,利用类似文丘里管装置使丝束扩散,并吸附到下部由输网帘和吸风系统组成的集合装置上,牵伸后的长丝靠风机的抽吸力均匀地沉积在输网帘上铺丝成网。
熔喷法工艺中,聚丙烯熔体由60°三角尖处的喷丝孔挤出,并立即受到三角两侧喷出的高温、高压热气流的牵伸,气流速度达到500~650m/s。挤出的聚丙烯熔体细流被迅速拉伸成超细纤维,在热牵伸气流波动下,牵伸后的超细纤维靠下方风机的抽吸均匀地分布在输网帘上。
c.成网
纺粘的纤网在网帘上形成第一层纤网,随后与熔喷纤网叠合形成双层纤网结构,再与纺粘纤网叠合形成三层纤网结构。叠合的三层纤网由输送帘输送至热轧粘合工序。
d.热轧加固
由输送帘将三层不同或相同纤网送至热轧机进行热粘合,热轧机通常由两根钢轧辊组成,其中一根为刻花辊,另一根为光辊。纤网在进入轧区时,受上下轧辊的温度、钳口压力和纤维的变形热作用,使纤网中的纤维相互熔融粘合,纤维网产生强度,再经冷却降温,可使纤维结构稳定。
e.卷绕
采用自动卷绕装置,自动控制卷绕张力,切边卷绕至一定长度或卷装直径时,卷绕机横切并自动换卷。
通过在SMS生产线上的多次试验与论证,依据本发明制备的SMS非织造布柔软度测试均优于常规产品。
附图说明
附图1为常规纺粘S流程简图、附图2为常规熔喷M流程简图、附
图3为常规SMS生产工艺流程简图。
具体实施方式
SMS原料包括以下重量比的材料:
1.PP纺粘树脂比例40-70%
等级:纺丝级熔体流动速率MFI(g/10min):14~75
2.熔喷树脂比例15-30%
常规熔喷树脂
等级:纺丝级熔体流动速率MFI(g/10min):300~1200
3.PP/PE共聚体的改性树脂比例10-30%
等级:纺丝级熔体流动速率MFI(g/10min):50~100
灰分含量(ppm):≤150结晶粒子(级):≤8
等规度(%):≥96分子量分布(MW/Mn):5
4.色母粒比例2-5%
等级:纺丝级熔体流动速率MFI(g/10min):15~50。
超柔SMS非织造布的制备方法包括以下步骤:
a.熔体准备与纺丝
聚丙烯树脂和熔喷用高熔融指数聚丙烯树脂以及添加相关的PP/PE共聚体的改性树脂通过自动输送系统输送到各自的储存料斗,与相关的添加剂按一定比例自动计量混和后进入螺杆挤压机,经挤压、熔融、计量,以一定的温度、压力进入熔体过滤器,除去杂质后,再经静态混和器进一步混和均匀,再经纺丝计量泵计量,进入纺丝组件过滤、混和、均匀后,由喷丝板喷出。
b.牵伸
纺粘冷却后的丝束被导入牵伸器,在牵伸器中心部延宽度方向有一牵伸槽,两侧吹入高压空气,丝束在牵伸槽中经高压空气牵伸后,利用类似文丘里管装置使丝束扩散,并吸附到下部由输网帘和吸风系统组成的集合装置上,牵伸后的长丝靠风机的抽吸力均匀地沉积在输网帘上铺丝成网。
熔喷法工艺中,聚丙烯熔体由60°三角尖处的喷丝孔挤出,并立即受到三角两侧喷出的高温、高压热气流的牵伸,气流速度达到500~650m/s。挤出的聚丙烯熔体细流被迅速拉伸成超细纤维,在热牵伸气流波动下,牵伸后的超细纤维靠下方风机的抽吸均匀地分布在输网帘上。
c.成网
纺粘的纤网在网帘上形成第一层纤网(S1),随后与熔喷纤网(M)叠合形成双层纤网结构,再与纺粘纤网(S2)叠合形成三层纤网结构。叠合的三层纤网由输送帘输送至热轧粘合工序。
d.热轧加固
由输送帘将三层不同或相同纤网送至热轧机进行热粘合,热轧机通常由两根钢轧辊组成,其中一根为刻花辊,另一根为光辊。纤网在进入轧区时,受上下轧辊的温度、钳口压力和纤维的变形热作用,使纤网中的纤维相互熔融粘合,纤维网产生强度,再经冷却降温,可使纤维结构稳定。
e.卷绕
采用自动卷绕装置,自动控制卷绕张力,切边卷绕至一定长
度或卷装直径时,卷绕机横切并自动换卷。
通过在SMS生产线上的多次试验与论证,依据本发明制备的SMS非织造布柔软度测试均优于常规产品。

Claims (2)

1.一种超柔SMS非织造布的制备方法,其特征是,SMS原料包括以下重量比的材料:PP纺粘树脂40-70%、熔喷树脂15-30%、PP/PE共聚体的改性树脂10-30%、色母粒2-5%。
2.权利要求1的一种超柔SMS非织造布的制备方法,其特征是,包括以下步骤:
a.熔体准备与纺丝
聚丙烯树脂和熔喷用高熔融指数聚丙烯树脂以及添加相关的PP/PE共聚体的改性树脂通过自动输送系统输送到各自的储存料斗,与相关的添加剂按一定比例自动计量混和后进入螺杆挤压机,经挤压、熔融、计量,以一定的温度、压力进入熔体过滤器,除去杂质后,再经静态混和器进一步混和均匀,再经纺丝计量泵计量,进入纺丝组件过滤、混和、均匀后,由喷丝板喷出。
b.牵伸
纺粘冷却后的丝束被导入牵伸器,在牵伸器中心部延宽度方向有一牵伸槽,两侧吹入高压空气,丝束在牵伸槽中经高压空气牵伸后,利用类似文丘里管装置使丝束扩散,并吸附到下部由输网帘和吸风系统组成的集合装置上,牵伸后的长丝靠风机的抽吸力均匀地沉积在输网帘上铺丝成网。
熔喷法工艺中,聚丙烯熔体由60°三角尖处的喷丝孔挤出,并立即受到三角两侧喷出的高温、高压热气流的牵伸,气流速度达到500~650m/s。挤出的聚丙烯熔体细流被迅速拉伸成超细纤维,在热牵伸气流波动下,牵伸后的超细纤维靠下方风机的抽吸均匀地分布在输网帘上。
c.成网
纺粘的纤网在网帘上形成第一层纤网,随后与熔喷纤网叠合形成双层纤网结构,再与纺粘纤网叠合形成三层纤网结构。叠合的三层纤网由输送帘输送至热轧粘合工序。
d.热轧加固
由输送帘将三层不同或相同纤网送至热轧机进行热粘合,热轧机通常由两根钢轧辊组成,其中一根为刻花辊,另一根为光辊。纤网在进入轧区时,受上下轧辊的温度、钳口压力和纤维的变形热作用,使纤网中的纤维相互熔融粘合,纤维网产生强度,再经冷却降温,可使纤维结构稳定。
e.卷绕
采用自动卷绕装置,自动控制卷绕张力,切边卷绕至一定长度或卷装直径时,卷绕机横切并自动换卷。
CN2011103842493A 2011-11-28 2011-11-28 超柔sms非织造布的制备方法 Pending CN102505348A (zh)