CN101991229B - 一种防湿透气鞋底及其制备方法 - Google Patents

一种防湿透气鞋底及其制备方法 Download PDF

Info

Publication number
CN101991229B
CN101991229B CN2010105258717A CN201010525871A CN101991229B CN 101991229 B CN101991229 B CN 101991229B CN 2010105258717 A CN2010105258717 A CN 2010105258717A CN 201010525871 A CN201010525871 A CN 201010525871A CN 101991229 B CN101991229 B CN 101991229B
Authority
CN
China
Prior art keywords
sole
water
sintering
percent
sodium chloride
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN2010105258717A
Other languages
English (en)
Other versions
CN101991229A (zh
Inventor
孙海云
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Dieshiqiao Investment Co.,Ltd.
Nantong Textile Capital Management Co ltd
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN2010105258717A priority Critical patent/CN101991229B/zh
Publication of CN101991229A publication Critical patent/CN101991229A/zh
Application granted granted Critical
Publication of CN101991229B publication Critical patent/CN101991229B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种由聚四氟乙烯为原料制成的防湿透气鞋底。由以下方法制成:制备模具;称取原料50-100目的聚四氟乙烯粉末50-65%,100-200目的氯化钠粉末15-25%,200-300目的白炭黑粉末5-10%,200-300目的石墨5-10%,0.1-0.5mm的玻璃纤维5-10%;压制,压力为50~60MPa,加压速率为10~15mm/min,保压5~10min;脱模烧结3-5小时,温度280-320℃;蒸煮10-20小时,换水2-4次。在原料中加入氯化钠,成型后用水将氯化钠溶解,在鞋底中留下若干个细小的孔,这种孔大个的水滴无法渗透进去,但水蒸气可以通过,使鞋底具有透气性,穿着舒适。

Description

一种防湿透气鞋底及其制备方法
技术领域
本发明涉及一种鞋底,特别涉及一种由聚四氟乙烯为原料制成的防湿透气鞋底。
背景技术
聚四氟乙烯俗称“塑料王”,具有优良的疏水性能,这种材料具有抗酸抗碱、抗各种有机溶剂的特点,几乎不溶于所有的溶剂,同时,聚四氟乙烯具有耐高温的特点。在固体材料中具有最小的表面张力,不粘附任何物质。因为其具有这么多优良的性质,故可以作为鞋底材料。但用聚四氟乙烯制成的鞋底,不具有透气性。
发明内容
本发明为了克服以上技术方面的不足,提供了一种即能防止水汽进入鞋内,又具有透气功能的防湿透气鞋底。
本发明是通过以下方式实现的。
一种防湿透气鞋底,其特征是采用以下方法制成:
(1)制备模具:按鞋底形状制备成压制模具;
(2)按以下重量百分比称取原料:
50-100目的聚四氟乙烯粉末       50-65%,
100-200目的氯化钠粉末          15-25%,
200-300目的白炭黑粉末          5-10%,
200-300目的石墨                5-10%,
0.1-0.5mm的玻璃纤维            5-10%;
(3)将上述原料混合均匀,加入模具内,用压力机进行压制,压制压力为50~60Mpa,加压速率为10~15mm/min,保压时间为5~10min;压好进行脱模;
(4)脱模后,放入烧结炉内烧结3-5小时,烧结温度为280-320℃,冷却至室温;
(5)烧结后,放入开水中蒸煮10-20小时,其间换水2-4次,使氯化钠浸入水中,制成防湿透气鞋底。
有益效果:在原料中加入氯化钠,成型后用水将氯化钠溶解,在鞋底中留下若干个细小的孔,这种孔大个的水滴无法渗透进去,但水蒸气可以通过,使鞋底具有透气性,穿着舒适。
具体实施方式:
实施例1
一种防湿透气鞋底,其特征是采用以下方法制成:
(1)制备模具:按鞋底形状制备成压制模具;
(2)按以下重量百分比称取原料:
50目的聚四氟乙烯粉末     50%,
100目的氯化钠粉末        20%,
200目的白炭黑粉末        10%,
200目的石墨              10%,
0.1mm的玻璃纤维          10%;
(3)将上述原料混合均匀,加入模具内,用压力机进行压制,压制压力为50Mpa,加压速率为10mm/min,保压时间为10min;压好进行脱模;
(4)脱模后,放入烧结炉内烧结3小时,烧结温度为280℃,冷却至室温;
(5)烧结后,放入开水中蒸煮20小时,其间换水4次,使氯化钠浸入水中,制成防湿透气鞋底。
实施例2
一种防湿透气鞋底,其特征是采用以下方法制成:
(1)制备模具:按鞋底形状制备成压制模具;
(2)按以下重量百分比称取原料:
100目的聚四氟乙烯粉末    65%,
200目的氯化钠粉末        17%,
300目的白炭黑粉末        5%,
300目的石墨              8%,
0.5mm的玻璃纤维          5%;
(3)将上述原料混合均匀,加入模具内,用压力机进行压制,压制压力为60Mpa,加压速率为15mm/min,保压时间为5min;压好进行脱模;
(4)脱模后,放入烧结炉内烧结5小时,烧结温度为320℃,冷却至室温;
(5)烧结后,放入开水中蒸煮10小时,其间换水2次,使氯化钠浸入水中,制成防湿透气鞋底。
透气性能及防水性能测试
根据上述实施例1的方法制备成聚四氟乙烯防湿透气鞋底,模具设定为1m2大,5mm的厚度,对照组也按照上述方法制备方法,只是在所用原料中把氯化钠去掉进行防水性与透气性的对比测试实验。
透气性能测试
透气性能通过透湿率来表征。取两个相同容量的大口杯,分别盛满相同量的水,将两种聚四氟乙烯鞋底分别覆盖在杯口上并固定,使杯内的水只能通过杯口处的聚四氟乙烯鞋底挥发出,分别称量两套装置的重量并记录。在大气相对湿度50%,温度21℃的条件下,测量每天通过覆盖在杯子上的聚四氟乙烯鞋底的水蒸气量,即透湿率。测得对照组透湿率为90克/平方米·天,本发明的聚四氟乙烯鞋底透湿率为1300克/平方米·天。可见,本发明提供的聚四氟乙烯鞋底比对照组的聚四氟乙烯鞋底在透气性能方面占很大优势。
防水性能测试
使用雨淋试验来测试防水性能。准备两块具有相同表面积、相同体积和重量的吸水板,分别垫在对照组聚四氟乙烯鞋底和本发明聚四氟乙烯鞋底后方,以相同压力的水流在距样品30cm处连续喷淋测试样,持续喷淋3个小时然后称量两块吸水板的重量。称量后发现,垫在对照组聚四氟乙烯鞋底后方的吸水板重量增加了0.11%,垫在本发明聚四氟乙烯鞋底后方的吸水板重量增加了0.16%,可见,本发明的聚四氟乙烯鞋底比对照组的聚四氟乙烯鞋底在防水性能方面只是稍有降低,但不会影响做成成品之后的防水性。

Claims (1)

1.一种防湿透气鞋底,其特征是采用以下方法制成:
(1)制备模具:按鞋底形状制备成压制模具;
(2)按以下重量百分比称取原料:
50-100目的聚四氟乙烯     50-65%,
100-200目的氯化钠        15-25%,
200-300目的白炭黑        5-10%,
200-300目的石墨          5-10%,
0.1-0.5mm的玻璃纤维      5-10%;
(2)将上述原料混合均匀,加入模具内,用压力机进行压制,压制压力为50~60Mpa,加压速率为10~15mm/min,保压时间为5~10min;压好进行脱模;
(3)脱模后,放入烧结炉内烧结3-5小时,烧结温度为280-320℃,冷却至室温;
(4)烧结后,放入开水中蒸煮10-20小时,其间换水2-4次,使氯化钠浸入水中,制成防湿透气鞋底。
CN2010105258717A 2010-11-01 2010-11-01 一种防湿透气鞋底及其制备方法 Active CN101991229B (zh)