CN101972653A - 一种锐钛矿型纳米Ag/TiO2复合材料的制备方法 - Google Patents

一种锐钛矿型纳米Ag/TiO2复合材料的制备方法 Download PDF

Info

Publication number
CN101972653A
CN101972653A CN 201010523692 CN201010523692A CN101972653A CN 101972653 A CN101972653 A CN 101972653A CN 201010523692 CN201010523692 CN 201010523692 CN 201010523692 A CN201010523692 A CN 201010523692A CN 101972653 A CN101972653 A CN 101972653A
Authority
CN
China
Prior art keywords
solution
silver
nano
crystal
tio
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 201010523692
Other languages
English (en)
Other versions
CN101972653B (zh
Inventor
杨辉
张璐璐
代春吉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shandong Xingchen Aluminum Technology Co., Ltd
Original Assignee
Shaanxi University of Science and Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shaanxi University of Science and Technology filed Critical Shaanxi University of Science and Technology
Priority to CN201010523692XA priority Critical patent/CN101972653B/zh
Publication of CN101972653A publication Critical patent/CN101972653A/zh
Application granted granted Critical
Publication of CN101972653B publication Critical patent/CN101972653B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种锐钛矿型纳米Ag/TiO2复合材料的制备方法,将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解后加入C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;继续搅拌加热至溶液蒸干,得白色固体;将白色固体连同烧杯一起置入烘箱中干燥后研细得粉体;将上述粉体于马弗炉中烧结得锐钛矿型纳米TiO2晶体。本发明载银是在纳米级的TiO2溶液中进行,混合比传统方法更加均匀,银与二氧化钛接触面积比现有方法中的大很多,载银不仅仅在表面进行,而是在所有的纳米二氧化钛颗粒中进行,降低了银的氧化变色程度,因而十分有利于得到银分散非常均匀、变色程度较小、催化活性和杀菌性能很强的纳米Ag/TiO2

Description

一种锐钛矿型纳米Ag/TiO2复合材料的制备方法
技术领域
本发明涉及一种纳米TiO2复合材料的制备方法,具体涉及一种锐钛矿型纳米Ag/TiO2复合材料的制备方法。
背景技术
锐钛矿相的TiO2是具有光催化特性的材料,它利用太阳光、荧光灯中的紫外光作激发源而具有净化空气、处理污水、自洁净等光催化效应和抗菌效应,且作用效果持久。其实现的前提是紫外光的激发,所以,在没有紫外光存在的场合,即使是锐钛矿相的TiO2也无光催化效果,以锐钛矿相的TiO2为载体的纳米载银二氧化钛复合材料(Ag/TiO2)因抗菌性很强的银离子的存在,在没有紫外线激发时也具有强的抑菌性和氧化性。研究表明:Ag作为光生电子的接收器可促进复合系统界面的载流子输运,使光生电子在金属表面积累,促使TiO2表面空穴增加,宽化TiO2对紫外线的吸收范围,大幅提高光催化氧化活性,且Ag+具有抗菌广谱性好、杀菌效率高、不易产生抗药性等特点。因此,纳米载银二氧化钛复合材料(Ag/TiO2)是理想的光催化材料和抗菌剂,不仅如此,这种材料有望催化光解水变成氢气和氧气的过程,其制备是目前人们研究的热点之一。
纳米载银二氧化钛复合材料的制备方法主要有:固相合成法、连续酸水解法和酸水解二次沉淀法,光还原沉积法、溶胶凝胶法、微波干燥等([1]柳清菊,张瑾,朱忠其等。载银TiO2无机抗菌剂的制备及性能研究。功能材料。2005.3(36):474~476;[2]马登峰,彭兵,柴立元等。载银纳米二氧化钛抗菌粉体的制备工艺研究。精细化工中间体。2006.2,36(1):63~66;[3]黄岳元,米钰,郭人民等。TiO2基纳米复合抗菌剂研究。化学工程。2004.8,32(4):46~48;[4]黄岳元,米钰,郭人民等。TiO2/Ag纳米抗菌材料。西北大学学报(自然科学版)2003.10,33(5):566~571;[5]刘雪峰,涂铭旌。稀土负载型纳米二氧化钛抗菌剂的研制。现代化工。2005.7,145~147;[6]刘雪峰,张利,涂铭旌。纳米Ce/TiO2无机抗菌剂的制备及其性能评价。过程工程学报。2004.6,4(3):256~260;[7]韩庆利1,金振兴,黄红艳。微波干燥制备Ag/TiO2的光催化活性试验研究。环境保护科学。2005.10,31(131):6~12;[8]章福祥,张秀,陈继新等。Ag/TiO2复合纳米催化剂的制备和表征及其光催化活性。催化学报。2003.11,24(11):887~880;[9]赵高凌,韩高荣。银钠米粒子P二氧化钛复合薄膜的溶胶凝胶法制备及其光学性质的研究。材料科学与工程。2001,19(1):21~25;[10]何进,陈星弼,杨传仁。TiO2(Ag)纳米半导体薄膜的制备及其光催化性能。电子元件与材料。1999,2:13~17;[11]王志群。复合型银系无机抗菌剂。申请专利号:98111623.X),这些方法基本制备过程分为两步:纳米二氧化钛粉体的制备和银离子的载入。制备中的水解过程消耗大量的酸,对连续水解法还需要在125℃下溶解偏钛酸,工艺操作过程复杂不易控制,生产成本高。
目前,制备纳米二氧化钛的专利亦有很多,但大多工艺复杂。申请号02120037的专利,制备过程中需特定波长范围的紫外灯光源的照射,且得到的钛溶胶还要经过老化,挥发溶剂,焙烧等过程;申请号200510070865的专利,水热合成后还要经过醇洗、水洗至中性,干燥等过程;申请号200910023823的专利,结合溶胶-凝胶和二次水解法制备锐钛矿型纳米二氧化钛,制备过程中需调节pH,然后滴加蒸馏水,连续搅拌得透明溶胶,陈化、干燥,再次加入蒸馏水,超声波振荡后静置、过滤、焙烧等过程。
发明内容
本发明的目的在于克服上述现有技术的缺点,提供了一种工艺简单、易操作、污染少、光吸收范围宽的锐钛矿型纳米Ag/TiO2复合材料的制备方法。
为达到上述目的,本发明采用的技术方案是:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量1%-5%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥0.5-1h后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为1%-5%的锐钛矿型纳米TiO2晶体。
本发明载银是在纳米级的TiO2溶液中进行,混合比传统方法更加均匀,银与二氧化钛接触面积比现有方法中的大很多,载银不仅仅在表面进行,而是在所有的纳米二氧化钛颗粒中进行,降低了银的氧化变色程度,因而十分有利于得到银分散非常均匀、变色程度较小、催化活性和杀菌性能很强的纳米Ag/TiO2;采用C16H36O4Ti作为原料,采用均匀热水解法得到了纯锐钛矿型的掺银晶体,与目前的固相合成法、连续酸水解法等所用的纳米TiO2或偏钛酸相比,原料价格便宜,可使生产成本大大降低,由于没有酸水解过程既可以降低成本又能减少酸污染,整个制备过程易于控制,工艺简单。
附图说明
图1为本发明所得Ag/TiO2晶体样品的XRD图谱和锐钛矿型TiO2晶体的标准图谱,结果表明:所示样品衍射峰与标准图谱吻合良好,没有杂峰出现,表明所得Ag/TiO2晶体是高纯度的锐钛矿型晶体;
图2为本发明所得Ag/TiO2晶体的TEM图,结果表明,纳米颗粒之间界面比较清楚,所得Ag/TiO2晶体为15-20纳米。
具体实施方式
实施例1:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量1%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥30分钟后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为1%的锐钛矿型纳米TiO2晶体。
实施例2:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量3%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥50分钟后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为3%的锐钛矿型纳米TiO2晶体。
实施例3:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量5%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥40分钟后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为5%的锐钛矿型纳米TiO2晶体。
实施例4:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量2%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥45分钟后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为2%的锐钛矿型纳米TiO2晶体。
实施例5:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量4%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥1小时后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为4%的锐钛矿型纳米TiO2晶体。
本发明的AgNO3氨溶液在锐钛矿型Ag/TiO2晶体制备中的作用是①提供晶体中的银元素;②使银离子在与TiO2共沉淀过程中缓慢均匀的进行,保证掺杂的均匀性;③TiO2沉淀时需在碱性条件下进行,AgNO3氨溶液为碱性溶液,因此,该溶液是TiO2的沉淀剂;④AgNO3氨溶液(Ag(NH3)2 +溶液)中有大量的未与银离子结合的NH3存在,可以与Ag/TiO2晶体表面裸露的离子形成络合物,因而对纳米颗粒起到分散剂的作用,是实现一步合成Ag/TiO2晶体的关键物质。
制备中搅拌条件保证了Ag(NH3)2 +和C16H36O4Ti两种溶液均匀的混合、同时控制沉淀时的过饱和度和晶体的生长;除去保鲜膜后搅拌主要目的是挥发除氨、降低溶液的pH值,使银氨络离子离解释放出Ag+,同时使Ag+通过离子交换或吸附进入到TiO2晶体中;550℃烧结处理目的在于得到结晶度高的锐钛矿型TiO2晶体。如烧结温度高于550℃则得到锐钛矿和金红石型二氧化钛的混合晶体。
本发明操作简单,不需酸水解过程,不消耗酸,污染小,成本低廉,易于工业化生产;所得材料为纳米载银二氧化钛复合材料,晶体组成全部为锐钛矿型TiO2,具有光催化作用;其粒度为15-20纳米,由于Ag+存在,其催化活性更高,在没有紫外线激发下仍然具有强氧化作用和杀菌作用。本发明产品即可作为强抗菌剂应用于多个领域,同时可用作强的光催化材料用于环境保护和洁净能源生产领域等。

Claims (1)

1.一种锐钛矿型纳米Ag/TiO2复合材料的制备方法,其特征在于:
1)取20ml质量百分比为25%的浓氨水于烧杯中,按掺杂量1%-5%将AgNO3加入浓氨水中,用保鲜膜封住杯口,在磁力搅拌器上加热搅拌使AgNO3完全溶解;
2)将步骤1)得到的溶液加热至剩余量为15ml时,再加入5ml的C16H36O4Ti,继续搅拌加热,溶液逐渐变为乳白色不透明溶液;
3)除去保鲜膜,继续搅拌加热至溶液蒸干,得白色固体;
4)将白色固体连同烧杯一起置入烘箱中于100℃干燥0.5-1h后研细得粉体;
5)将上述粉体于200℃的马弗炉中烧结2h,除去晶体中残存的含氮物质和水,再于550℃的马弗炉中烧结3h,使晶体进一步结晶化,最后得到银离子掺杂量为1%-5%的锐钛矿型纳米TiO2晶体。
CN201010523692XA 2010-10-27 2010-10-27 一种锐钛矿型纳米Ag/TiO2复合材料的制备方法 Active CN101972653B (zh)