WO2026023348A1 - バリアフィルム、積層体及び包装袋 - Google Patents
バリアフィルム、積層体及び包装袋Info
- Publication number
- WO2026023348A1 WO2026023348A1 PCT/JP2025/023539 JP2025023539W WO2026023348A1 WO 2026023348 A1 WO2026023348 A1 WO 2026023348A1 JP 2025023539 W JP2025023539 W JP 2025023539W WO 2026023348 A1 WO2026023348 A1 WO 2026023348A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- film
- resin layer
- polyamide
- mass
- resin
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
- B29C65/00—Joining or sealing of preformed parts, e.g. welding of plastics materials; Apparatus therefor
- B29C65/02—Joining or sealing of preformed parts, e.g. welding of plastics materials; Apparatus therefor by heating, with or without pressure
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/32—Layered products comprising a layer of synthetic resin comprising polyolefins
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/34—Layered products comprising a layer of synthetic resin comprising polyamides
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B9/00—Layered products comprising a layer of a particular substance not covered by groups B32B11/00 - B32B29/00
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B65—CONVEYING; PACKING; STORING; HANDLING THIN OR FILAMENTARY MATERIAL
- B65D—CONTAINERS FOR STORAGE OR TRANSPORT OF ARTICLES OR MATERIALS, e.g. BAGS, BARRELS, BOTTLES, BOXES, CANS, CARTONS, CRATES, DRUMS, JARS, TANKS, HOPPERS, FORWARDING CONTAINERS; ACCESSORIES, CLOSURES, OR FITTINGS THEREFOR; PACKAGING ELEMENTS; PACKAGES
- B65D65/00—Wrappers or flexible covers; Packaging materials of special type or form
- B65D65/38—Packaging materials of special type or form
- B65D65/40—Applications of laminates for particular packaging purposes
-
- C—CHEMISTRY; METALLURGY
- C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
- C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
- C23C14/00—Coating by vacuum evaporation, by sputtering or by ion implantation of the coating forming material
- C23C14/06—Coating by vacuum evaporation, by sputtering or by ion implantation of the coating forming material characterised by the coating material
- C23C14/08—Oxides
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
- Y02W—CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT
- Y02W30/00—Technologies for solid waste management
- Y02W30/50—Reuse, recycling or recovery technologies
- Y02W30/80—Packaging reuse or recycling, e.g. of multilayer packaging
Definitions
- This disclosure relates to barrier films, laminates, and packaging bags.
- Flexible packaging materials are made by laminating multiple films. Films made from polyesters such as polyethylene terephthalate are used to give the packaging material strength and heat resistance, films made from polyamide 6 are used to give it pinhole resistance, and films made from polypropylene are used to give it strength and water vapor barrier properties. These films are usually biaxially oriented, making them suitable for printing.
- the biaxially stretched film is printed as needed, and an unstretched film, usually made of unstretched polyethylene or polypropylene, is laminated to the printed surface.
- unstretched polyethylene or polypropylene film is placed on the inside, and the insides are heat-sealed to create a packaging bag from a laminate of multiple films.
- a layer of aluminum foil, aluminum, alumina, or silicon oxide vapor-deposited film, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, or the like is placed between the biaxially stretched film and the unstretched film.
- Flexible packaging materials can be made by layering several different materials to meet the required performance and be used to package a variety of contents.
- mono-materialization which means making flexible packaging materials recyclable.
- Polyolefins, which are easily recyclable, are considered to be the preferred mono-material materials.
- Packaging bags for heat sterilization are filled with the contents, sealed, and then boiled or retorted. Heated contents may also be filled into the bags. Because these processes involve heat treatment of the packaging bags, it is more appropriate to use polypropylene, which has better heat resistance than polyethylene, for the unstretched film that is heat-sealed to seal.
- polypropylene which has better heat resistance than polyethylene
- the polypropylene film is endowed with properties suitable for packaging, such as printability, barrier properties, heat-sealability, and lamination. Printing is performed on strong biaxially oriented polypropylene film. Heat-sealing is performed using unstretched polypropylene film.
- Patent Document 1 lists polyamide as a resin material having a melting point of 180°C or higher.
- amorphous aromatic polyamide which is a polyamide resin containing a certain amount of isophthalic acid units as a constituent unit, is easily formed into a film. Therefore, in order to improve film formability, it is considered to use amorphous aromatic polyamide as a resin material having a melting point of 180°C or higher.
- some barrier films which have a layer containing an amorphous aromatic polyamide on one side of a polypropylene film and an inorganic oxide vapor-deposited on the surface of this layer, have poor retort resistance, such as a decrease in barrier properties after retort treatment.
- the present inventors have found that, in a layer containing an amorphous aromatic polyamide provided on one side of a polypropylene film, by adjusting the proportion of the number of aromatic diamine units within a certain range while maintaining the content of amorphous aromatic polyamide at a certain level or higher, and by vapor-depositing an inorganic oxide on the surface of this layer, it is possible to obtain a barrier film that has excellent retort resistance while improving film formability.
- acid-modified polypropylene is a highly adhesive polypropylene-based resin, and have discovered that by providing a layer containing acid-modified polypropylene between a polypropylene film and a layer containing polyamide, it is possible to suppress interlayer delamination without impairing recyclability.
- the present disclosure has been completed based on these findings and through further investigation.
- a barrier film having a vapor-deposited film on the first resin layer side of a polymer film includes the first resin layer, the second resin layer, and the third resin layer in this order;
- the first resin layer constitutes one outermost layer of the polymer film, the first resin layer contains a polyamide resin, and the polyamide resin contains an aromatic polyamide;
- a ratio of the number of diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer is 85 mol% or more;
- a ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer is 15 mol% or more and 70 mol% or less;
- the content of the amorphous aromatic polyamide in the first resin layer is 25% by mass or more;
- the second resin layer contains an acid-modified polypropylene, the third resin layer
- the polyamide resin contained in the first resin layer is two types of polyamide, i.e., a first polyamide and a second polyamide; the first polyamide is the amorphous aromatic polyamide, The barrier film according to ⁇ 1>, wherein the second polyamide is a crystalline aromatic polyamide.
- the polyamide resin contained in the first resin layer is a first polyamide, a second polyamide, and a third polyamide; the first polyamide is the amorphous aromatic polyamide, the second polyamide is a crystalline aromatic polyamide, The barrier film according to ⁇ 1>, wherein the third polyamide is an aliphatic polyamide.
- ⁇ 4> ⁇ 3> The barrier film according to ⁇ 3>, wherein the content of the third polyamide in the first resin layer is 1% by mass or more and 75% by mass or less.
- ⁇ 5> ⁇ 4> The barrier film according to any one of ⁇ 2> to ⁇ 4>, wherein the content of the first polyamide in the first resin layer is 25% by mass or more and 95% by mass or less.
- ⁇ 6> ⁇ 5> The barrier film according to any one of ⁇ 2> to ⁇ 5>, wherein the content of the second polyamide in the first resin layer is 5% by mass or more and 75% by mass or less.
- the polymer film has a polypropylene content of 70% by mass or more.
- the third resin layer has the largest thickness among the first resin layer, the second resin layer, and the third resin layer;
- ⁇ 10> The barrier film according to any one of ⁇ 1> to ⁇ 9>, further comprising a barrier coating layer on the vapor-deposited film side.
- ⁇ 11> ⁇ 10> A laminate comprising the barrier film according to any one of ⁇ 1> to ⁇ 10> and a heat sealant film.
- the laminate includes a polypropylene substrate film on the barrier film opposite the heat sealant film, ⁇ 11> or ⁇ 12>, wherein the laminate has a water-welded peel strength of 0.3 N/15 mm or more when the film containing the polypropylene base film is peeled from the film containing the barrier film and the heat sealant film in accordance with JIS K 6854-2:1999 after retort treatment at 121°C and 0.2 MPa for 30 minutes.
- the laminate includes a polypropylene substrate film on the barrier film opposite the heat sealant film
- ⁇ 16> The packaging bag according to ⁇ 15>, wherein a water-welded peel strength when the film containing the polypropylene base film and the film containing the barrier film and the heat sealant film are peeled off in accordance with JIS K 6854-2:1999 is 0.3 N/15 mm or more.
- the present disclosure can provide a barrier film that can suppress delamination and has excellent film-forming properties, recyclability, and retort resistance.
- the present disclosure also provides a laminate and a packaging bag using the barrier film.
- FIG. 1 is a schematic cross-sectional view showing one embodiment of a polymer film used in the present disclosure.
- FIG. 2 is a schematic cross-sectional view showing another embodiment of a polymer film used in the present disclosure.
- 1 is a schematic cross-sectional view illustrating one embodiment of a barrier film according to the present disclosure.
- FIG. FIG. 2 is a schematic cross-sectional view showing another embodiment of a barrier film according to the present disclosure.
- FIG. 1 is a schematic cross-sectional view of an embodiment of a barrier film according to the present disclosure, in which a barrier coat layer is provided.
- 1 is a schematic cross-sectional view showing one embodiment of a laminate according to the present disclosure.
- FIG. 2 is a schematic cross-sectional view showing another embodiment of a laminate according to the present disclosure.
- FIG. 1 is a graph showing the change in tensile stress with respect to the distance between a pair of grippers that pull two films together to measure peel strength.
- 1 is a front view showing one embodiment
- the numerical range of the parameter may be constructed by combining any one upper limit candidate value with any one lower limit candidate value.
- the numerical range of parameter B may be A1 or more and A4 or less, A1 or more and A5 or less, A1 or more and A6 or less, A2 or more and A4 or less, A2 or more and A5 or less, A2 or more and A6 or less, A3 or more and A4 or less, A3 or more and A5 or less, or A3 or more and A6 or less.
- polymer film A schematic cross-sectional view of a polymer film 10 used in the barrier film of the present disclosure is shown in Figure 1.
- the polymer film 10 comprises a first resin layer 11, a second resin layer 12, and a third resin layer 13, in this order.
- the first resin layer 11 constitutes one of the outermost layers of the polymer film 10.
- the third resin layer 13 constitutes the other outermost layer of the polymer film 10.
- FIG 2 shows a schematic cross-sectional view of another embodiment of a polymer film 10 used in the barrier film of the present disclosure.
- the polymer film 10 comprises, in this order, a first resin layer 11, a second resin layer 12, a third resin layer 13, and a fourth resin layer 14.
- the first resin layer 11 constitutes one of the outermost layers of the polymer film 10.
- the fourth resin layer 14 constitutes the other outermost layer of the polymer film 10.
- a vapor-deposited film 15 is provided on the first resin layer side of the polymer film 10 to form the barrier film of the present disclosure.
- the surface roughness Sa of one outermost surface of the polymer film 10 is preferably 0.10 ⁇ m or less, more preferably 0.07 ⁇ m or less, even more preferably 0.05 ⁇ m or less, and is preferably 0.01 ⁇ m or more, more preferably 0.02 ⁇ m or more, and even more preferably 0.03 ⁇ m or more.
- the surface roughness Sa of one outermost surface of the polymer film 10 is preferably 0.01 ⁇ m or more and 0.10 ⁇ m or less, more preferably 0.02 ⁇ m or more and 0.07 ⁇ m or less, and even more preferably 0.03 ⁇ m or more and 0.05 ⁇ m or less.
- the surface roughness Sa of the other outermost surface of the polymer film 10 is preferably 0.20 ⁇ m or less, more preferably 0.17 ⁇ m or less, even more preferably 0.14 ⁇ m or less, and preferably 0.05 ⁇ m or more, more preferably 0.07 ⁇ m or more, and even more preferably 0.09 ⁇ m or more.
- the surface roughness Sa of the other outermost surface of the polymer film 10 is preferably 0.05 ⁇ m or more and 0.20 ⁇ m or less, more preferably 0.07 ⁇ m or more and 0.17 ⁇ m or less, and even more preferably 0.09 ⁇ m or more and 0.14 ⁇ m or less.
- the first resin layer 11 contains a polyamide resin, and the polyamide resin contains an aromatic polyamide.
- the aromatic polyamide is a polyamide resin containing a benzene ring.
- aromatic polyamides include copolymers of aromatic diamines and aliphatic dicarboxylic acids, copolymers of aliphatic diamines and dicarboxylic acids containing a benzene ring, copolymers of aromatic diamines and dicarboxylic acids containing a benzene ring, copolymers of aromatic diamines and aliphatic dicarboxylic acids further copolymerized with at least one selected from the group consisting of aliphatic diamines and dicarboxylic acids containing a benzene ring, and copolymers of aliphatic diamines and dicarboxylic acids further copolymerized with at least one selected from the group consisting of aromatic diamines and aliphatic carboxylic acids.
- Two or more types of diamines
- Aromatic diamines are diamines containing a benzene ring, such as metaxylenediamine, paraxylenediamine, metaphenylenediamine, and paraphenylenediamine. One or more of these may be used.
- Dicarboxylic acids containing a benzene ring include aromatic dicarboxylic acids such as terephthalic acid (TPA) and isophthalic acid (IPA), and naphthalenedicarboxylic acids such as 1,2-naphthalenedicarboxylic acid, 1,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid. One or more of these may be used.
- aromatic dicarboxylic acids such as terephthalic acid (TPA) and isophthalic acid (IPA)
- naphthalenedicarboxylic acids such as 1,2-
- the first resin layer 11 may contain an aliphatic polyamide as the polyamide resin.
- Aliphatic polyamide is a polyamide resin that does not contain a benzene ring. Examples of aliphatic polyamides include polyamides 6, 7, 10, 11, 12, 410, 56, 66, 69, 610, 611, 612, and 1010. The first resin layer 11 may contain one or more of these.
- the first resin layer 11 may contain resins other than polyamide, such as polyester, acrylic resin, or ionomer resin, as long as this does not affect processability or physical properties.
- Aminocarboxylic acid units are structural units of ring-opening polymerization polyamides.
- Dicarboxylic acid units are one of the structural units of copolymer polyamides.
- the "total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer” corresponds to the total amount (moles) of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer, and represents the total amount of polyamide resin constituting the first resin layer.
- the number of "diamine units contained in the aromatic polyamide” corresponds to the amount (moles) of diamine units contained in the aromatic polyamide, and represents the amount of aromatic polyamide.
- the "ratio of the number of diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer” represents the proportion of aromatic polyamides in the total amount of polyamide resin constituting the first resin layer.
- a method for theoretically calculating the ratio of the number of diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer will be described below with an example.
- the ratio of the number of diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer is 100 mol %.
- the polyamide resin constituting the first resin layer is composed of 5% by mass of polyamide 6 and 95% by mass of polyamide 6I (a copolymer of 1,6-hexanediamine and isophthalic acid).
- the retort resistance of the barrier film is improved.
- the ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer is 15 mol% or more, preferably 18 mol% or more, more preferably 21 mol% or more, even more preferably 24 mol% or more, and is 70 mol% or less, preferably 50 mol% or less, more preferably 40 mol% or less, even more preferably 30 mol% or less.
- the ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer is 15 mol% or more and 70 mol% or less, preferably 18 mol% or more and 50 mol% or less, more preferably 21 mol% or more and 40 mol% or less, and even more preferably 24 mol% or more and 30 mol% or less.
- the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer represents the amount of all polyamide resins constituting the first resin layer, and therefore "the ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer” is an index showing the degree to which aromatic diamine units are contained in all polyamide resins constituting the first resin layer.
- MXD6 contains equal numbers of meta-xylenediamine units (-NH-CH 2 -C 6 H 4 -CH 2 -NH-, molecular weight 134) as diamine units and adipic acid units (-CO-(CH 2 ) 4 -CO-, molecular weight 112) as dicarboxylic acid units.
- 1 H-NMR spectrum is measured, and the ratio of the number of each amino carboxylic acid unit and the ratio of the number of each diamine unit in the first resin layer are calculated, whereby “the ratio of the number of diamine units in the aromatic polyamide to the total number of amino carboxylic acid units and diamine units in the polyamide resin constituting the first resin layer" and “the ratio of the number of aromatic diamine units in the aromatic polyamide to the total number of amino carboxylic acid units and diamine units in the polyamide resin constituting the first resin layer” can be determined.
- the protons from which the peaks observed in the 1H -NMR spectrum are derived can be identified by comparing the results with those of the 1H -NMR spectrum of known polyamide resins, etc. From the area ratios of the respective peaks, the proportions of the numbers of the respective aminocarboxylic acid units and the respective diamine units contained in the first resin layer can be determined.
- the 1 H-NMR spectrum is measured in the same manner as when a measurement sample is prepared from a polymer film and the 1 H-NMR spectrum is measured.
- the 1 H-NMR spectrum is measured as follows.
- the laminate was cut into small pieces with scissors, freeze-pulverized, and then placed in a sample vial.
- a 1:1 mixed solvent of chloroform and formic acid was added to the sample vial, which was then placed in an ultrasonic cleaner for 10 minutes and allowed to stand overnight.
- the organic solvent phase is filtered through a chromatographic disc with a filter pore size of 0.45 ⁇ m, and concentrated and dried using a nitrogen blower. 10 mL of chloroform is added to the dried product, and the mixture is placed in an ultrasonic cleaner for 2 to 3 minutes.
- the mixture is then filtered through 5C filter paper, and the filtered product is washed with chloroform.
- the filtered material together with the filter paper of 5C is dried with a nitrogen blow, then the filtered material is dissolved in formic acid, and the filtrate is recovered.
- the recovered filtrate is dried with a nitrogen blow and used as a measurement sample. Thereafter, the 1 H-NMR spectrum is measured in the same manner as above.
- Aromatic polyamides are classified into crystalline aromatic polyamides and amorphous aromatic polyamides.
- amorphous polyamide means a polyamide that does not have a clear melting point, specifically, a polyamide having a crystalline melting enthalpy ⁇ Hm of 5 J/g or less, preferably 3 J/g or less, more preferably 1 J/g or less.
- crystalline polyamide means a polyamide that has a well-defined melting point, specifically a polyamide whose crystalline melting enthalpy ⁇ Hm is greater than 5 J/g.
- the crystalline fusion enthalpy is obtained by differential scanning calorimetry (DSC) in accordance with JIS K 7121:2012 and JIS K 7122:2012.
- Examples of the crystalline aromatic polyamide include a copolymer of metaxylenediamine and adipic acid, and a copolymer of metaxylenediamine and adipic acid and isophthalic acid.
- Examples of the copolymer of metaxylenediamine with adipic acid and isophthalic acid include a copolymer of metaxylenediamine with a dicarboxylic acid in which the molar ratio of adipic acid/isophthalic acid is 93/7, and a copolymer of metaxylenediamine with a dicarboxylic acid in which the molar ratio of adipic acid/isophthalic acid is 8/2.
- amorphous aromatic polyamides examples include copolymers of 1,6-hexanediamine and isophthalic acid, copolymers of metaxylenediamine and isophthalic acid, copolymers of 1,6-hexanediamine and isophthalic acid and terephthalic acid, copolymers of metaxylenediamine and adipic acid and isophthalic acid, copolymers of 1,6-hexanediamine and metaxylenediamine and adipic acid and isophthalic acid, copolymers of 2-methyl-1,5-pentanediamine and isophthalic acid and terephthalic acid, and copolymers of 2,2,4-trimethylhexamethylenediamine and terephthalic acid.
- the content of the amorphous aromatic polyamide in the first resin layer is 25% by mass or more, preferably 40% by mass or more, more preferably 55% by mass or more, and even more preferably 70% by mass or more.
- the content of the amorphous aromatic polyamide in the first resin layer is equal to or greater than the lower limit, film formability is improved.
- the upper limit of the content of the amorphous aromatic polyamide in the first resin layer is 100% by mass.
- the content of the amorphous aromatic polyamide in the first resin layer is preferably 25% by mass or more and 100% by mass or less, more preferably 40% by mass or more and 100% by mass or less, even more preferably 55% by mass or more and 100% by mass or less, and even more preferably 70% by mass or more and 100% by mass or less.
- the polyamide resin contained in the first resin layer may be one type or two or more types.
- the ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer can be adjusted within the above range by appropriately adjusting the type and ratio of monomers used in synthesizing the polyamide resin.
- the ratio of the number of aromatic diamine units contained in the aromatic polyamide to the total number of aminocarboxylic acid units and diamine units contained in the polyamide resin constituting the first resin layer can be adjusted to 15 mol% to 70 mol%.
- the polyamide resin contained in the first resin layer is two types of polyamide resin, a first polyamide and a second polyamide, will be described.
- the first resin layer contains an amorphous aromatic polyamide as the polyamide resin
- the first polyamide is an amorphous aromatic polyamide.
- the second polyamide may be an amorphous aromatic polyamide, a crystalline aromatic polyamide, or an aliphatic polyamide.
- the content of the first polyamide in the first resin layer is preferably 25% by mass or more and 95% by mass or less, more preferably 40% by mass or more and 85% by mass or less, even more preferably 55% by mass or more and 75% by mass or less, and still more preferably 70% by mass or more and 75% by mass or less.
- the content of the second polyamide in the first resin layer is preferably 5% by mass or more, more preferably 15% by mass or more, even more preferably 25% by mass or more, and is 75% by mass or less, preferably 60% by mass or less, more preferably 45% by mass or less, even more preferably 30% by mass or less.
- the thickness of the barrier coat layer 16 is preferably 0.01 ⁇ m or more and 10 ⁇ m or less, more preferably 0.1 ⁇ m or more and 5 ⁇ m or less, and even more preferably 0.2 ⁇ m or more and 1 ⁇ m or less.
- the barrier coating layer 16 can be formed by dissolving or dispersing the gas barrier resin in water or a suitable solvent, applying the solution, and drying it.
- the barrier coat layer 16 is preferably a gas barrier coating film containing at least one resin composition, such as a metal alkoxide hydrolysate or a metal alkoxide hydrolysis condensate, obtained by polycondensing a mixture of a metal alkoxide and a water-soluble polymer by the sol-gel method in the presence of a sol-gel catalyst, water, an organic solvent, etc.
- the gas barrier coating film is a gas barrier coating film of a mixture of a metal alkoxide and a water-soluble polymer, or a gas barrier coating film of a mixture of a metal alkoxide, a water-soluble polymer, and a silane coupling agent.
- Examples of the metal atom M that can be used include silicon, zirconium, titanium, and aluminum.
- Examples of the organic group represented by R1 and R2 include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and an i-butyl group.
- metal alkoxides that satisfy the above general formula include tetramethoxysilane (Si(OCH 3 ) 4 ), tetraethoxysilane (Si(OC 2 H 5 ) 4 ), tetrapropoxysilane (Si(OC 3 H 7 ) 4 ), and tetrabutoxysilane (Si(OC 4 H 9 ) 4 ).
- a silane coupling agent may be used together with the metal alkoxide.
- silane coupling agents include known organic reactive group-containing organoalkoxysilanes, such as vinyltrimethoxysilane, ⁇ -chloropropylmethyldimethoxysilane, ⁇ -chloropropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyltriethoxysilane, ⁇ -methacryloxypropyltrimethoxysilane, ⁇ -methacryloxypropylmethyldimethoxysilane, and 1,3,5-tris(3-methoxysilylpropyl)isocyanurate.
- organoalkoxysilanes such as vinyltrimethoxysilane, ⁇ -chloropropylmethyldimethoxys
- silane coupling agents Two or more types may be used, and it is preferable to use the silane coupling agent in an amount within the range of 1 part by mass to 20 parts by mass per 100 parts by mass of the total amount of the metal alkoxide.
- Preferred water-soluble polymers are polyvinyl alcohol and ethylene-vinyl alcohol copolymers, and from the standpoints of oxygen barrier properties, water vapor barrier properties, water resistance, and weather resistance, it is preferable to use these in combination.
- the degree of polymerization of polyvinyl alcohol is preferably 300 or more, which can prevent deterioration of gas barrier properties due to bending.
- the degree of polymerization of polyvinyl alcohol is preferably 3000 or less, which can prevent processing from becoming difficult.
- the degree of polymerization of polyvinyl alcohol is preferably 300 or more and 3,000 or less.
- the degree of saponification of polyvinyl alcohol is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more.
- the barrier film of the present disclosure is formed into a laminate by providing a barrier coat layer 16 on the surface of a vapor-deposited film 15 and laminating it with another film.
- a polymer film 10 having a first resin layer 11, a second resin layer 12, and a third resin layer 13 has a vapor-deposited film 15 on the first resin layer side of the barrier film, and the barrier coat layer 16 is provided on the surface of the vapor-deposited film 15 of the barrier film. It is also possible to laminate the surface of the vapor-deposited film 15 with another film without providing the barrier coat layer 16.
- the barrier film of the present disclosure is formed into a laminate by providing a barrier coat layer 16 on the vapor-deposited film 15 surface and laminating it with another film.
- the barrier film has a vapor-deposited film 15 on the first resin layer 11 side of a polymer film 10 having a first resin layer 11, a second resin layer 12, a third resin layer 13, and a fourth resin layer 14, and the barrier coat layer 16 is provided on the vapor-deposited film 15 surface of the barrier film. It is also possible to laminate the vapor-deposited film 15 surface with another film without providing the barrier coat layer 16.
- the heat sealant film 18 is primarily composed of polypropylene with a melting point of 120°C or higher, which improves the heat resistance of the packaging material. There are no particular restrictions on the polypropylene, as long as it has a melting point of 120°C or higher. In this specification, "polyolefin with a melting point of 120°C or higher” refers to polypropylene whose maximum peak temperature in DSC is 120°C or higher.
- the thickness of the adhesive layer 17 is not particularly limited and can be, for example, 0.1 ⁇ m or more and 10 ⁇ m or less.
- the resulting packaging bags are filled with food, seasonings, beverages, supplements, pharmaceuticals, enteral nutrients, pet food, etc., and then sealed.
- the sealed packaging bags are then subjected to boiling or retort processing.
- a heat-sterilized food pouch is a packaging bag that contains food as its contents and has been subjected to a heat sterilization process.
- Figure 9 shows a front view of one embodiment of the packaging bag.
- the packaging bag 30 has a storage section 37 that stores the contents. The configuration of the packaging bag 30 will be described below.
- the width direction of the packaging bag 30 is also referred to as the first direction D1.
- the pair of side portions 33 described above face each other in the first direction D1.
- the direction perpendicular to the first direction D1 is also referred to as the second direction D2.
- the packaging bag 30 of this embodiment is intended to be used in such a way that the consumer opens the packaging bag 30 by tearing it along the first direction D1.
- the packaging bag 30 includes a surface laminate 34 that forms the surface, and a back laminate 35 that forms the back.
- the seal portion has an outer edge seal portion that extends along the outer edge of the packaging bag 30.
- the outer edge seal portion includes a lower seal portion 32a that extends along the lower portion 32, and a pair of side seal portions 33a that extend along a pair of side portions 33.
- the lower seal portion 32a, side seal portion 33a, and upper seal portion 31a are seal portions formed by joining the inner surface of the front laminate 34 and the inner surface of the back laminate 35.
- the seal may be formed by melting the inner surfaces of the laminates by heating or the like, welding the inner surfaces together, i.e., by heat sealing.
- the seal may be formed by bonding the inner surfaces of opposing laminates together using an adhesive or the like.
- the surface laminate 34 and the back laminate 35 may be provided with easy-open means 25 for tearing the surface laminate 34 and the back laminate 35 along the first direction D1 to open the packaging bag 30.
- the easy-open means 25 may include a notch 26 formed in the side seal portion 33a of the packaging bag 30, which serves as a tearing starting point.
- the easy-open means 25 may include a half-cut line formed by laser processing, a cutter, or the like, in the portion that serves as a path for tearing the packaging bag 30.
- the water-wet peel strength when the film containing the polypropylene base film is peeled from the film containing the barrier film and the heat sealant film in accordance with JIS K 6854-2: 1999 is preferably 0.3 N/15 mm or more, more preferably 0.5 N/15 mm or more, even more preferably 1.0 N/15 mm or more, and still more preferably 2.0 N/15 mm or more.
- the water-wet peel strength is equal to or greater than the lower limit, peeling between layers or cohesive peeling within layers can be suppressed.
- a test piece is prepared by cutting the laminate constituting the packaging bag 30 so that the long side direction of the test piece coincides with the width direction (first direction D1) of the packaging bag 30, as shown by reference symbol 80A in Fig. 9 .
- a test piece is also prepared by cutting the laminate constituting the packaging bag 30 so that the long side direction of the test piece coincides with the direction perpendicular to the width direction of the packaging bag 30 (second direction D2), as shown by reference symbol 80B in Fig. 9 .
- the water-wet peel strengths of the two test pieces are then measured using a tensile tester.
- the smaller measured value is the water-wet peel strength when the film containing the polypropylene base film is peeled from the film containing the barrier film and the heat sealant film in the laminate constituting the heat-sterilized food pouch.
- the specific method for measuring the water-wet peel strength of the test piece is the same as above.
- polyamide resins used in the following experimental examples are as follows: Polyamide A Amorphous aromatic polyamide: Copolymer of 1,6-hexanediamine and dicarboxylic acid with a molar ratio of isophthalic acid/terephthalic acid of 7/3. Polyamide B Crystalline aromatic polyamide: Polyamide C, a copolymer of metaxylenediamine and a dicarboxylic acid with a molar ratio of adipic acid/isophthalic acid of 93/7.
- Crystalline aromatic polyamide Polyamide D, a copolymer of metaxylenediamine and adipic acid Aliphatic polyamide Homopolymer of 6-aminohexanoic acid unit Synthesized by ring-opening polymerization of ⁇ -caprolactam
- Example 1-1 As the resin (first resin) constituting the first resin layer, a mixture of 75% by mass of polyamide A and 25% by mass of polyamide B was used. As the resin (second resin) constituting the second resin layer, an acid-modified polypropylene random copolymer (ethylene-1-butene-propylene random copolymer graft-polymerized with 1.2 mol% maleic anhydride, MFR: 5.0) was used. As the resin (third resin) constituting the third resin layer, homopolypropylene (MFR: 3.0) was used. As the resin (fourth resin) constituting the fourth resin layer, an ethylene-1-butene-propylene random copolymer (MFR: 5.3) was used.
- MFR ethylene-1-butene-propylene random copolymer
- the first resin, the second resin, the third resin, and the fourth resin were co-extruded, and then stretched 5.0 times in the longitudinal direction (MD direction) and 10.0 times in the transverse direction (TD direction) using a sequential biaxial stretching device, to produce a polymer film of Experimental Example 1-1 comprising a first resin layer (0.7 ⁇ m), a second resin layer (1.0 ⁇ m), a third resin layer (17.0 ⁇ m), and a fourth resin layer (1.3 ⁇ m).
- the thickness of the polymer film in Experimental Example 1-1 was 20 ⁇ m.
- the polypropylene content in the entire polymer film of Experimental Example 1-1 was 95% by mass.
- Example 1-2 A polymer film of Experimental Example 1-2 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 70% by mass of polyamide A and 30% by mass of polyamide B was used as the first resin.
- Example 1-3 A polymer film of Experimental Example 1-3 was produced in the same manner as the polymer film of Experimental Example 1-2, except that the thickness of the first resin layer was set to 0.1 ⁇ m. The thickness of the polymer film in Experimental Example 1-3 was 19.4 ⁇ m. The polypropylene content in the entire polymer film of Experimental Example 1-3 was 99% by mass.
- Example 1-4 A polymer film of Experimental Example 1-4 was produced in the same manner as the polymer film of Experimental Example 1-2, except that the thickness of the first resin layer was set to 5.0 ⁇ m. The thickness of the polymer film in Experimental Example 1-4 was 24.3 ⁇ m. The polypropylene content in the entire polymer film of Experimental Example 1-4 was 74% by mass.
- Example 1-5 A polymer film of Experimental Example 1-5 was produced in the same manner as the polymer film of Experimental Example 1-2, except that the thickness of the first resin layer was set to 0.4 ⁇ m. The thickness of the polymer film in Experimental Example 1-5 was 19.7 ⁇ m. The polypropylene content in the entire polymer film of Experimental Example 1-5 was 97% by mass.
- Example 1-6 A polymer film of Experimental Example 1-6 was produced in the same manner as the polymer film of Experimental Example 1-2, except that the thickness of the first resin layer was 1.5 ⁇ m. The thickness of the polymer film in Experimental Example 1-6 was 20.8 ⁇ m. The polypropylene content in the entire polymer film of Experimental Example 1-6 was 91% by mass.
- Example 1-7 As the resin (first resin) constituting the first resin layer, a mixture of 70% by mass of polyamide A and 30% by mass of polyamide B was used. As the resin (second resin) constituting the second resin layer, an acid-modified polypropylene random copolymer (ethylene-1-butene-propylene random copolymer graft-polymerized with 1.2 mol% maleic anhydride, MFR: 5.0) was used. As the resin (third resin) constituting the third resin layer, homopolypropylene (MFR: 3.0) was used.
- the first resin, the second resin, the third resin, the fourth resin, and the fifth resin were co-extruded, and then stretched 5.0 times in the longitudinal direction (MD direction) and 10.0 times in the transverse direction (TD direction) using a sequential biaxial stretching device, to produce a polymer film of Experimental Example 1-7 having a first resin layer (0.7 ⁇ m), a second resin layer (1.0 ⁇ m), a third resin layer (17.0 ⁇ m), a fourth resin layer (1.0 ⁇ m), and a fifth resin layer (0.7 ⁇ m) in this order.
- the thickness of the polymer film in Experimental Example 1-7 was 20.4 ⁇ m.
- the polypropylene content in the entire polymer film of Experimental Example 1-7 was 91% by mass.
- Example 1-8 A polymer film of Experimental Example 1-8 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 70% by mass of polyamide A and 30% by mass of polyamide C was used as the first resin.
- Example 1-11 A polymer film of Experimental Example 1-11 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 50% by mass of polyamide A and 50% by mass of polyamide B was used as the first resin.
- Example 1-12 A polymer film of Experimental Example 1-12 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 35% by mass of polyamide A and 65% by mass of polyamide B was used as the first resin.
- Example 1-13 A polymer film of Experimental Example 1-13 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 35% by mass of polyamide A and 65% by mass of polyamide C was used as the first resin.
- Example 1-14 The polymer film of Experimental Example 1-14 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 35% by mass of polyamide A, 59% by mass of polyamide C, and 6% by mass of polyamide D was used as the first resin.
- Example 1-15 A polymer film of Experimental Example 1-15 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 80% by mass of polyamide A and 20% by mass of polyamide D was used as the first resin.
- Example 1-16 A polymer film of Experimental Example 1-16 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 75% by mass of polyamide A and 25% by mass of polyamide D was used as the first resin.
- Example 1-17 A polymer film of Experimental Example 1-17 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 20% by mass of polyamide A and 80% by mass of polyamide C was used as the first resin.
- Example 1-18 A polymer film of Experimental Example 1-18 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 20% by mass of polyamide A and 80% by mass of polyamide B was used as the first resin.
- Example 1-19 A polymer film of Experimental Example 1-19 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 30% by mass of polyamide A and 70% by mass of polyamide D was used as the first resin.
- Example 1-20 A polymer film of Experimental Example 1-20 was produced in the same manner as the polymer film of Experimental Example 1-1, except that a mixture of 20% by mass of polyamide A and 80% by mass of polyamide D was used as the first resin.
- Example 1-21 A polymer film of Experimental Example 1-21 was produced in the same manner as the polymer film of Experimental Example 1-2, except that a mixture of 95% by mass of ethylene-1-butene-propylene random copolymer (MFR: 5.3) and 5% by mass of high-density polyethylene (MFR: 1.1) was used as the fourth resin.
- MFR ethylene-1-butene-propylene random copolymer
- MFR high-density polyethylene
- Example 1-22 A polymer film of Experimental Example 1-22 was produced in the same manner as Experimental Example 1-11, except that homopolypropylene (MFR: 3.0) was used as the fourth resin.
- MFR homopolypropylene
- Example 1-23 A polymer film of Experimental Example 1-23 was produced in the same manner as Experimental Example 1-18, except that homopolypropylene (MFR: 3.0) was used as the fourth resin.
- a polymer film of Experimental Example 1-23 was produced in the same manner as the polymer film of Experimental Example 1-22, except that a mixture of 20% by mass of polyamide A and 80% by mass of polyamide B was used as the first resin.
- Example 1-24 A polymer film of Experimental Example 1-24 was produced in the same manner as the polymer film of Experimental Example 1-2, except that instead of stretching 5.0 times in the longitudinal direction (MD direction), the film was stretched 4.7 times in the longitudinal direction (MD direction), and the amount of resin extruded was adjusted so that the thicknesses of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer after stretching were 0.7 ⁇ m, 1.0 ⁇ m, 17.0 ⁇ m, and 1.3 ⁇ m, respectively.
- Example 1-25 A polymer film of Experimental Example 1-25 was produced in the same manner as the polymer film of Experimental Example 1-2, except that instead of stretching 5.0 times in the longitudinal direction (MD direction), the film was stretched 4.5 times in the longitudinal direction (MD direction), and the amount of resin extruded was adjusted so that the thicknesses of the first resin layer, the second resin layer, the third resin layer, and the fourth resin layer after stretching were 0.7 ⁇ m, 1.0 ⁇ m, 17.0 ⁇ m, and 1.3 ⁇ m, respectively.
- the peaks derived from protons observed in the 1 H-NMR spectrum measurement of the standard sample prepared from each pellet were assigned, and the proportion of the number of each amino carboxylic acid unit and the proportion of the number of each diamine unit were calculated from the area ratio of each peak, thereby calculating the proportion of the number of diamine units to the total number of amino carboxylic acid units and diamine units, and the proportion of the number of aromatic diamine units to the total number of amino carboxylic acid units and diamine units, respectively.
- the objective lens of a laser microscope (Keyence Corporation, measurement unit model number VK-X160, control unit model number VK-X150) was set to 50x, zoom to 1x, measurement quality to ultra-high speed, pitch to 0.13 ⁇ m, and double scan to none.
- the field of view at this time was 203.555 ⁇ m ⁇ 271.495 ⁇ m.
- the polymer film fixed to the slide glass was placed under the objective lens so that the vertical direction (MD direction) and the short side direction of the field of view were parallel.
- a connection range of 1 in the short side direction x 5 in the long side direction was specified, and the upper and lower limits of the scan height and brightness were manually adjusted appropriately to obtain three connected images of five connected images in the horizontal direction (TD direction).
- the size of the connected image was 200 ⁇ 5 ⁇ m x 1220 ⁇ 10 ⁇ m.
- a numerical value of 0.5 mm was specified for waviness removal in surface shape correction, and waviness was removed.
- surface roughness measurement the entire area of each connected image was specified, and the surface roughness Sa was calculated. The average of the three calculated values was taken as the surface roughness Sa of one of the outermost layers.
- the other outermost layer (the surface of the fourth resin layer in Experimental Examples 1-1, 1-2, 1-5, 1-6, 1-8 to 1-21, and 1-24 to 1-26, and the surface of the fifth resin layer in Experimental Example 1-7) was also measured in the same manner to calculate the surface roughness Sa, and the average of the three calculated values was used as the surface roughness Sa of the fourth resin layer.
- Winding property evaluation Each of the polymer films of Experimental Examples 1-1 to 1-26 was wound up after film formation and evaluated based on the following evaluation criteria. A: No wrinkles were generated during winding. B: Wrinkles occurred during winding, and film production and winding had to be stopped.
- Example 2-1 The polymer film of Experimental Example 1-1 was introduced into the unwinding compartment of a decompressible chamber having an unwinding compartment, a plasma treatment compartment, a film formation compartment, a winding compartment, etc., and the chamber was decompressed.
- a plasma treatment apparatus the surface of the first resin layer of the polymer film of Experimental Example 1-1 was subjected to plasma pretreatment using a mixed gas of argon and oxygen at a volume ratio of 1:1 in a roll-to-roll manner while applying tension to the polymer film of Experimental Example 1-1.
- a resistance heating method was used as an aluminum heating means to vapor-deposit aluminum while introducing oxygen, thereby forming an aluminum oxide (alumina) vapor-deposited film with a thickness of 10 nm (PVD method).
- a barrier coating agent was prepared on the surface of the vapor-deposited film in the following manner to form a barrier coating layer.
- 385 g of water, 67 g of isopropyl alcohol, and 9.1 g of 0.5 N hydrochloric acid were mixed to prepare a solution with a pH of 2.2.
- 175 g of tetraethoxysilane as a metal alkoxide was mixed into this solution while cooling to 10° C., thereby obtaining solution A.
- Solution B was obtained by mixing 14.7 g of polyvinyl alcohol as a water-soluble polymer having a saponification degree of 99% or more and a polymerization degree of 2400, 324 g of water, and 17 g of isopropyl alcohol.
- Solution A and solution B were mixed at a mass ratio of 5.5:4.5 to obtain a barrier coating agent.
- the barrier coating agent was coated on the surface of the vapor-deposited film and dried at 100°C for 10 seconds.
- the thickness of the barrier coating layer formed by drying the barrier coating agent was 300 nm. In this manner, a barrier film of Experimental Example 2-1 was produced.
- Example 2-2 A barrier film of Experimental Example 2-2 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-2 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-3 A barrier film of Experimental Example 2-3 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-8 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-4 A barrier film of Experimental Example 2-4 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-9 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-5 A barrier film of Experimental Example 2-5 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-10 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-6 A barrier film of Experimental Example 2-6 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-11 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-7 A barrier film of Experimental Example 2-7 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-12 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-8 A barrier film of Experimental Example 2-8 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-13 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-9 A barrier film of Experimental Example 2-9 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-14 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-10 A barrier film of Experimental Example 2-10 was produced in the same manner as in Experimental Example 2-2, except that the formation of the vapor-deposited film was changed as follows.
- the surface of the first resin layer of the polymer film of Experimental Example 1-2 was subjected to plasma pretreatment using a mixed gas of argon and oxygen in a volume ratio of 1:1.
- Silicon oxide was vapor-deposited on the plasma-treated surface using an electron beam heating method as heating means and silicon monoxide as a vapor deposition source to form a silicon oxide vapor-deposited film with a thickness of 30 nm (PVD method).
- Example 2-11 A barrier film of Experimental Example 2-11 was produced in the same manner as in Experimental Example 2-10, except that the barrier coat layer was not formed.
- Example 2-12 A barrier film of Experimental Example 2-12 was produced in the same manner as in Experimental Example 2-11, except that a silicon oxide vapor-deposited film having a thickness of 30 nm was formed on the surface of the first resin layer of the polymer film of Experimental Example 1-2 without performing plasma pretreatment.
- Example 2-13 A barrier film of Experimental Example 2-13 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-21 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-14 A barrier film of Experimental Example 2-14 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-5 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-15 A barrier film of Experimental Example 2-15 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-6 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-16 A barrier film of Experimental Example 2-16 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-24 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-17 A barrier film of Experimental Example 2-17 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-25 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-18 A barrier film of Experimental Example 2-18 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-26 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-19 A barrier film of Experimental Example 2-19 was produced in the same manner as Experimental Example 2-10, except that the polymer film of Experimental Example 1-12 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-20 A barrier film of Experimental Example 2-20 was produced in the same manner as in Experimental Example 2-19, except that the barrier coat layer was not formed.
- Example 2-21 A barrier film of Experimental Example 2-21 was produced in the same manner as in Experimental Example 2-2, except that the formation of the vapor-deposited film was changed as follows.
- a carbon-containing silicon oxide vapor deposition film having a thickness of 30 nm was formed on the surface of the first resin layer of the polymer film of Experimental Example 1-2 by roll-to-roll deposition using a plasma chemical vapor deposition apparatus (plasma CVD apparatus) while applying tension to the polymer film of Experimental Example 1-2.
- plasma CVD apparatus plasma chemical vapor deposition apparatus
- Example 2-22 A barrier film of Experimental Example 2-22 was produced in the same manner as in Experimental Example 2-21, except that the barrier coat layer was not formed.
- Example 2-23 A barrier film of Experimental Example 2-23 was produced in the same manner as Experimental Example 2-21, except that the polymer film of Experimental Example 1-12 was used instead of the polymer film of Experimental Example 1-2.
- Example 2-24 A barrier film of Experimental Example 2-24 was produced in the same manner as in Experimental Example 2-23, except that the barrier coat layer was not formed.
- Example 2-25 A barrier film of Experimental Example 2-25 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-15 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-26 A barrier film of Experimental Example 2-26 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-16 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-27 A barrier film of Experimental Example 2-27 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-17 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-28 A barrier film of Experimental Example 2-28 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-18 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-29 A barrier film of Experimental Example 2-29 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-19 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-30 A barrier film of Experimental Example 2-30 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-20 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-31 A barrier film of Experimental Example 2-31 was produced in the same manner as in Experimental Example 2-2, except that the formation of the vapor-deposited film was changed as follows.
- the surface of the first resin layer of the polymer film of Experimental Example 1-2 was subjected to plasma pretreatment using a mixed gas of argon and oxygen in a volume ratio of 1:1.
- a 30 nm thick aluminum vapor deposition film was formed on the plasma-treated surface using conventional vacuum metallization technology.
- Example 2-32 A barrier film of Experimental Example 2-32 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-22 was used instead of the polymer film of Experimental Example 1-1.
- Example 2-33 A barrier film of Experimental Example 2-33 was produced in the same manner as Experimental Example 2-1, except that the polymer film of Experimental Example 1-23 was used instead of the polymer film of Experimental Example 1-1.
- Test pieces were obtained by cutting out the barrier films of Experimental Examples 2-1 to 2-33. Using these test pieces, the oxygen permeability (unit: cc/( m2 day atm)) and water vapor permeability (unit: g/( m2 day)) were measured by the following methods.
- oxygen permeability unit: cc/( m2 day atm)
- water vapor permeability unit: g/( m2 day)
- Oxygen permeability Using an oxygen permeability measuring device (OX-TRAN2/20 manufactured by MOCON Corporation), the test piece was set so that the polymer film side was the oxygen supply side, and the oxygen permeability was measured in an environment of a temperature of 23°C and a relative humidity of 90% RH in accordance with JIS K 7126-2:2006.
- a biaxially oriented polypropylene film with a thickness of 20 ⁇ m was prepared as the polypropylene substrate film.
- a urethane-based printing ink was applied to one side of the polypropylene substrate film by gravure roll coating to form a printed layer.
- the dried thickness of the printed layer was 1 ⁇ m.
- the polypropylene substrate film with the printed layer formed thereon will be referred to as the printed film.
- the printed layer of the printed film and the surface of the barrier coat layer of the barrier film of Experimental Example 2-1 were bonded together using a two-component curing polyurethane adhesive.
- the thickness of the adhesive layer formed by the two-component curing polyurethane adhesive was 2 ⁇ m.
- a 60 ⁇ m thick unstretched polypropylene film was prepared as a heat sealant film.
- the surface of the fourth resin layer of the barrier film of Experimental Example 2-1 was bonded to the heat sealant film using a two-component curing polyurethane adhesive.
- the thickness of the adhesive layer formed by the two-component curing polyurethane adhesive was 2 ⁇ m. In this way, a laminate was produced. Laminates were similarly produced using the barrier films of Experimental Examples 2-2 to 2-33 instead of the barrier film of Experimental Example 2-1.
- Test pieces were obtained by cutting out the laminates prepared from the barrier films of Experimental Examples 2-1 to 2-33. The oxygen permeability and water vapor permeability of these test pieces were measured in the same manner as above.
- Laminates prepared from the barrier films of Experimental Examples 2-1 to 2-33 were cut into A4 size, folded in half at the long edge, with the heat sealant film facing the other side, and three sides, including the folded portion, were heat-sealed at a width of 7 mm to prepare three-sided sealed packaging bags.
- This packaging bag was filled with 200 mL of tap water, and the remaining side was heat-sealed to form a retort packaging bag filled with the contents.
- the retort packaging bag was subjected to a high-temperature retort treatment using steam at 135°C and 0.3 MPa for 30 minutes.
- a laminate was cut out from the retort packaging bag after the high-temperature retort treatment, and the oxygen permeability and water vapor permeability were measured in the same manner as above.
- a 297 mm x 210 mm laminate was cut from the retort pouch after the high-temperature retort treatment, and a flex load (stroke: 155 mm, flexion angle: 440°) was applied 10 times using a Gelbo Flex Tester (manufactured by Tester Sangyo Co., Ltd.) in accordance with ASTM F 392. After the flex load, the oxygen permeability and water vapor permeability of the laminate were measured in the same manner as described above.
- Experimental Examples 2-1 to 2-33 are shown in Tables 6 to 11.
- Experimental Examples 2-25 to 2-30 and 2-33 are comparative examples.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Mechanical Engineering (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Materials Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- Laminated Bodies (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2026528500A JPWO2026023348A1 (cg-RX-API-DMAC7.html) | 2024-07-23 | 2025-06-30 |
Applications Claiming Priority (4)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2024-118254 | 2024-07-23 | ||
| JP2024118254 | 2024-07-23 | ||
| JP2025015282 | 2025-01-31 | ||
| JP2025-015282 | 2025-01-31 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2026023348A1 true WO2026023348A1 (ja) | 2026-01-29 |
Family
ID=98565355
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2025/023539 Pending WO2026023348A1 (ja) | 2024-07-23 | 2025-06-30 | バリアフィルム、積層体及び包装袋 |
Country Status (2)
| Country | Link |
|---|---|
| JP (1) | JPWO2026023348A1 (cg-RX-API-DMAC7.html) |
| WO (1) | WO2026023348A1 (cg-RX-API-DMAC7.html) |
Citations (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH07144394A (ja) * | 1993-11-25 | 1995-06-06 | Sumitomo Bakelite Co Ltd | 複合多層フィルム |
| JP2000158610A (ja) * | 1998-11-27 | 2000-06-13 | Sumitomo Bakelite Co Ltd | 複合シート及び密封容器 |
| JP2008023779A (ja) * | 2006-07-19 | 2008-02-07 | Mitsubishi Gas Chem Co Inc | 多層構造物 |
| JP2011214089A (ja) | 2010-03-31 | 2011-10-27 | Dainippon Printing Co Ltd | 蒸着フィルム製造方法 |
| JP2012035504A (ja) * | 2010-08-06 | 2012-02-23 | Mitsubishi Gas Chemical Co Inc | 多層容器 |
| JP2012076292A (ja) | 2010-09-30 | 2012-04-19 | Dainippon Printing Co Ltd | ガスバリア性フィルム積層体 |
| WO2013002070A1 (ja) * | 2011-06-27 | 2013-01-03 | 三菱瓦斯化学株式会社 | フィルム及びフィルム包装容器 |
| WO2018083962A1 (ja) * | 2016-11-04 | 2018-05-11 | 三菱瓦斯化学株式会社 | 易裂性アルミ蒸着二軸延伸フィルム |
| WO2019087960A1 (ja) | 2017-10-30 | 2019-05-09 | 大日本印刷株式会社 | 積層フィルム、バリア性積層フィルム及び該バリア性積層フィルムを用いたガスバリア性包装材料、ガスバリア性包装体 |
| JP2019177909A (ja) * | 2018-03-30 | 2019-10-17 | 出光ユニテック株式会社 | 包装体 |
| JP2022007964A (ja) | 2020-03-31 | 2022-01-13 | 大日本印刷株式会社 | 積層体、レトルト用またはボイル用パウチ |
| JP2023020735A (ja) * | 2021-07-30 | 2023-02-09 | 大日本印刷株式会社 | 蒸着フィルム、積層体、包装材料及び包装容器 |
| JP2023020738A (ja) * | 2021-07-30 | 2023-02-09 | 大日本印刷株式会社 | 樹脂基材、印刷基材、蒸着フィルム、積層体、包装材料及び包装容器 |
| JP2023118613A (ja) * | 2022-02-15 | 2023-08-25 | 大日本印刷株式会社 | 積層体、包装材料用積層体及び包装容器 |
-
2025
- 2025-06-30 JP JP2026528500A patent/JPWO2026023348A1/ja active Pending
- 2025-06-30 WO PCT/JP2025/023539 patent/WO2026023348A1/ja active Pending
Patent Citations (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH07144394A (ja) * | 1993-11-25 | 1995-06-06 | Sumitomo Bakelite Co Ltd | 複合多層フィルム |
| JP2000158610A (ja) * | 1998-11-27 | 2000-06-13 | Sumitomo Bakelite Co Ltd | 複合シート及び密封容器 |
| JP2008023779A (ja) * | 2006-07-19 | 2008-02-07 | Mitsubishi Gas Chem Co Inc | 多層構造物 |
| JP2011214089A (ja) | 2010-03-31 | 2011-10-27 | Dainippon Printing Co Ltd | 蒸着フィルム製造方法 |
| JP2012035504A (ja) * | 2010-08-06 | 2012-02-23 | Mitsubishi Gas Chemical Co Inc | 多層容器 |
| JP2012076292A (ja) | 2010-09-30 | 2012-04-19 | Dainippon Printing Co Ltd | ガスバリア性フィルム積層体 |
| WO2013002070A1 (ja) * | 2011-06-27 | 2013-01-03 | 三菱瓦斯化学株式会社 | フィルム及びフィルム包装容器 |
| WO2018083962A1 (ja) * | 2016-11-04 | 2018-05-11 | 三菱瓦斯化学株式会社 | 易裂性アルミ蒸着二軸延伸フィルム |
| WO2019087960A1 (ja) | 2017-10-30 | 2019-05-09 | 大日本印刷株式会社 | 積層フィルム、バリア性積層フィルム及び該バリア性積層フィルムを用いたガスバリア性包装材料、ガスバリア性包装体 |
| JP2019177909A (ja) * | 2018-03-30 | 2019-10-17 | 出光ユニテック株式会社 | 包装体 |
| JP2022007964A (ja) | 2020-03-31 | 2022-01-13 | 大日本印刷株式会社 | 積層体、レトルト用またはボイル用パウチ |
| JP2023020735A (ja) * | 2021-07-30 | 2023-02-09 | 大日本印刷株式会社 | 蒸着フィルム、積層体、包装材料及び包装容器 |
| JP2023020738A (ja) * | 2021-07-30 | 2023-02-09 | 大日本印刷株式会社 | 樹脂基材、印刷基材、蒸着フィルム、積層体、包装材料及び包装容器 |
| JP2023118613A (ja) * | 2022-02-15 | 2023-08-25 | 大日本印刷株式会社 | 積層体、包装材料用積層体及び包装容器 |
Also Published As
| Publication number | Publication date |
|---|---|
| JPWO2026023348A1 (cg-RX-API-DMAC7.html) | 2026-01-29 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7594742B2 (ja) | 積層体、レトルト用またはボイル用パウチ | |
| JP2024050712A (ja) | 積層体および包装容器 | |
| JP7818189B2 (ja) | 包装袋 | |
| JP7649487B2 (ja) | 多層基材、該多層基材を備える多層フィルム、該多層フィルムを備える積層体および該積層体を備える包装材料 | |
| JP7594744B2 (ja) | 多層基材、該多層基材を備える多層フィルム、該多層フィルムを備える積層体および該積層体を備える包装材料 | |
| JP7658063B2 (ja) | 積層体および包装容器 | |
| JP2024107175A (ja) | 基材、蒸着基材、積層体および包装容器 | |
| JP2024107177A (ja) | 蒸着基材、積層体および包装容器 | |
| JP2024107186A (ja) | 積層体および包装容器 | |
| JP2000127286A (ja) | バリア性フィルムおよびそれを使用した積層材 | |
| WO2026023340A1 (ja) | バリアフィルム、積層体及び包装袋 | |
| WO2026023345A1 (ja) | 高分子フィルム、バリアフィルム、積層体及び包装袋 | |
| WO2026023344A1 (ja) | 高分子フィルム、バリアフィルム、積層体及び包装袋 | |
| JP2024177010A (ja) | 延伸基材、バリア性基材、積層体および包装容器 | |
| JP2024052534A (ja) | バリア性基材、積層体および包装容器 | |
| JP2025021847A (ja) | 2軸延伸ポリエチレンフィルム | |
| WO2026023346A1 (ja) | 高分子フィルム、バリアフィルム、積層体及び包装袋 | |
| JP2025021850A (ja) | 延伸基材、バリア性基材、積層体および包装容器 | |
| JP2025021853A (ja) | 延伸基材、バリア性基材、積層体および包装容器 | |
| JP2025141864A (ja) | バリア性フィルム、積層体および包装容器 | |
| WO2024252688A1 (ja) | 延伸基材、印刷基材、バリア性基材、積層体および包装容器 | |
| JP2024177011A (ja) | 延伸基材、バリア性基材、積層体および包装容器 | |
| JP2025141863A (ja) | バリア性フィルム、積層体および包装容器 | |
| JP2024177008A (ja) | 延伸基材、バリア性基材、積層体および包装容器 | |
| JP2024177009A (ja) | 延伸基材、バリア性基材、積層体および包装容器 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 25844443 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2026528500 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2026528500 Country of ref document: JP |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 25844443 Country of ref document: EP |