WO2024105967A1 - 高強度極厚鋼板およびその製造方法 - Google Patents

高強度極厚鋼板およびその製造方法 Download PDF

Info

Publication number
WO2024105967A1
WO2024105967A1 PCT/JP2023/031503 JP2023031503W WO2024105967A1 WO 2024105967 A1 WO2024105967 A1 WO 2024105967A1 JP 2023031503 W JP2023031503 W JP 2023031503W WO 2024105967 A1 WO2024105967 A1 WO 2024105967A1
Authority
WO
WIPO (PCT)
Prior art keywords
less
plate thickness
thickness
strength
rolling
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/031503
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
智久 矢野
直樹 ▲高▼山
俊一 橘
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Steel Corp
Original Assignee
JFE Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JFE Steel Corp filed Critical JFE Steel Corp
Priority to JP2023573540A priority Critical patent/JP7468814B1/ja
Priority to CN202380059615.9A priority patent/CN119630827A/zh
Priority to KR1020257004200A priority patent/KR20250034987A/ko
Publication of WO2024105967A1 publication Critical patent/WO2024105967A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/04—Ferrous alloys, e.g. steel alloys containing manganese
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0221—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the working steps
    • C21D8/0226—Hot rolling
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0247—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment
    • C21D8/0263—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment following hot rolling
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/001—Ferrous alloys, e.g. steel alloys containing N
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/02—Ferrous alloys, e.g. steel alloys containing silicon
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/06—Ferrous alloys, e.g. steel alloys containing aluminium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
    • C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
    • C22C38/58—Ferrous alloys, e.g. steel alloys containing chromium with nickel with more than 1.5% by weight of manganese
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/002—Bainite
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/005—Ferrite

Definitions

  • the present invention relates to a high-strength extra-thick steel plate with a thickness of over 100 mm that is used in large structures such as ships, marine structures, low-temperature storage tanks, architectural structures, and civil engineering structures, and that has excellent brittle crack propagation arrest properties, and to a method for manufacturing the same.
  • Ni content in steel has been known as a means of improving the brittle crack arrestability of steel materials.
  • 9% Ni steel is used on a commercial scale in liquefied natural gas (LNG) storage tanks, which require brittle crack arrestability at extremely low temperatures.
  • LNG liquefied natural gas
  • increasing the amount of Ni in steel necessitates a significant increase in manufacturing costs, making it difficult to apply to applications other than LNG storage tanks.
  • the TMCP Thermo-Mechanical Control Process
  • Patent Document 1 discloses a technology that enhances brittle crack propagation arrestability by improving toughness through a microstructure that is a mixed structure of ferrite and bainite, or a mixed structure of ferrite, pearlite and bainite, and by controlling the average crystal grain size in the center of the plate thickness to 5 to 20 ⁇ m.
  • Patent Document 2 a technique for ultra-fine-graining the structure of the surface layer of the steel material is disclosed, for example, in Patent Document 2 and Patent Document 3.
  • Patent Document 2 attention is paid to the fact that a shear lip (i.e., a plastic deformation region) that occurs in the surface layer of a steel material when a brittle crack propagates is effective in improving the brittle crack propagation arrest property.
  • Patent Document 2 discloses that the crystal grains in the shear lip portion are refined so that the propagation energy of the propagating brittle crack is absorbed by the crystal grains.
  • Patent Document 2 discloses a manufacturing method in which a process is repeated one or more times to cool the surface layer portion to a temperature below the Ar3 transformation point by controlled cooling after hot rolling, and then stop the controlled cooling and reheat the surface layer portion to a temperature above the Ar3 transformation point.
  • Patent Document 2 discloses that in this process, a roll reduction is applied to the steel material to repeatedly cause transformation or work recrystallization, thereby generating an ultrafine ferrite structure or bainite structure in the surface layer portion.
  • Patent Document 3 discloses that in order to improve the brittle crack propagation arrest properties of steel material with a microstructure mainly composed of ferrite-pearlite, both surface portions of the steel material are composed of layers having a ferrite structure with ferrite grains having a circular equivalent grain size of 5 ⁇ m or less and an aspect ratio of 2 or more at 50% or more by area, while suppressing the variation in ferrite grain size.
  • Patent Document 3 discloses that the maximum reduction rate per pass during finish rolling is set to 12% or less to suppress local recrystallization phenomena.
  • Patent Document 4 the average equivalent circle diameter of effective crystal grains is 25 ⁇ m or less in the surface layer portion of a thick steel plate and 35 ⁇ m or less in the center portion of the plate thickness, and the texture intensity ratio with respect to the rolling surface and rolling direction is as follows: I ⁇ 001 ⁇ 110>+I ⁇ 112 ⁇ 110>+I ⁇ 332 ⁇ 113>>5, I ⁇ 110 ⁇ 001>+I ⁇ 110 ⁇ 110>+I ⁇ 001 ⁇ 010> ⁇ 3 and at the center of the plate thickness, I ⁇ 001 ⁇ 110>+I ⁇ 112 ⁇ 110>+I ⁇ 332 ⁇ 113> ⁇ 3.5
  • the texture is controlled so as to satisfy the following:
  • Patent Document 4 discloses a technique for improving the brittle crack propagation arrestability by controlling the texture so as to satisfy the following:
  • Patent Document 5 the steel plate is divided into three layers: a front and back layer extending from the front and back sides in the thickness direction up to 25%; and the remaining central portion of the plate thickness.
  • a front and back layer extending from the front and back sides in the thickness direction up to 25%; and the remaining central portion of the plate thickness.
  • an area of 5% to 25% of the plate thickness has a texture in which the (100) X-ray plane intensity ratio parallel to the rolling surface is 1.5 or more and less than 2.0, and in the central portion of the plate thickness, a texture in which the (111) and/or (211) X-ray plane intensity ratio parallel to the rolling surface is 2.0 or more is controlled.
  • Patent Document 5 discloses a technology that improves brittle crack propagation arrest properties in this way.
  • Patent Documents 2 and 3 involve cooling only the surface layer of the steel material, then reheating it, and processing it during reheating to obtain a specific structure. This means that it is difficult to control on an actual production scale, and there are problems with the large load placed on the rolling and cooling equipment.
  • Patent Documents 1 to 5 are primarily intended for steel plates and steel materials with a thickness of approximately 80 mm, and it is unclear whether the specified characteristics can be obtained when applying each technology to extra-thick steel plates over 100 mm. It is also unclear whether the characteristics required for stopping crack propagation in the plate thickness direction, which are required in hull structures, can be obtained. However, it is predicted that the characteristics required to stop crack propagation will be higher for extra-thick steel plates over 100 mm compared to steel plates with a thickness of approximately 80 mm.
  • the present invention was made in consideration of the above problems, and aims to provide a high-strength, extra-thick steel plate that has excellent toughness and brittle crack propagation arrest properties, even when the plate thickness exceeds 100 mm, and a manufacturing method thereof.
  • high strength in the present invention refers to a yield strength (YS) of 390 MPa or more at 1/2 the plate thickness position of a high-strength extra thick steel plate.
  • Excellent toughness in the present invention refers to a Charpy fracture transition temperature of vTrs ⁇ -100°C at 1/2 the plate thickness position of a high-strength extra thick steel plate.
  • Excellent brittle crack propagation arrestability (arrestability)” in the present invention refers to a Kca value at -10°C (hereinafter also referred to as Kca(-10°C) value (N/mm3 /2 )) of 8400 N/mm3 /2 or more.
  • the yield strength, vTrs and Kca values can be measured by the methods described in the Examples below.
  • the inventors have conducted extensive research into high-strength, extra-thick steel plates that have excellent toughness and brittle crack propagation arrest properties while maintaining strength even when the plate thickness is over 100 mm, and into a manufacturing method for stably obtaining such steel plates. As a result, they have obtained the following findings.
  • the hot rolling process is controlled so that the cumulative reduction in the austenite non-recrystallization temperature range is 50.0% or more, the reduction ratio is 3.25 or more, and the rolling end temperature at the 1/2 thickness position is Ar3 or more.
  • This control effectively refines the crystal grains of the steel structure at the 1/2 thickness position and controls the texture at the 1/2 thickness position. This makes it possible to achieve excellent low-temperature toughness while elongating the austenite in the rolling direction and developing a bainite transformation texture in a specific direction. As a result, a texture is obtained in which the X-ray intensity of the (211) plane on the rolled surface at the 1/2 thickness position is 1.60 or more.
  • the present invention has been completed based on the above findings and further investigations, and the gist of the present invention is as follows.
  • C 0.040 to 0.150%, Si: 0.02 to 0.50%, Mn: 1.00 to 2.50%, P: 0.020% or less, S: 0.010% or less, Al: 0.010 to 0.100%, N: 0.0010 to 0.0100% or less, O: 0.0100% or less, and Ceq defined by formula (1) is 0.480 to 0.560%, with the balance being Fe and unavoidable impurities;
  • the X-ray intensity ratio of the (211) plane on the rolled surface at the 1/2 position of the sheet thickness is 1.60 or more,
  • the steel structure at the 1/2 position of the plate thickness is a mixed structure consisting of 80 to 100% bainite phase and 0 to 20% ferrite phase, in terms of area fraction, the average grain size of bainite crystal grains surrounded by grain boundaries with an orientation difference of 15° or more is 20 ⁇ m or less, and the circle equivalent diameter of the maximum
  • Ceq C + Mn/6 + Cu/15 + Ni/15 + Cr/5 + Mo/5 + V/5 ...
  • C, Mn, Cu, Ni, Cr, Mo and V in formula (1) represent the content (mass %) of each element, and the content of an element that is not contained is set to 0.
  • Group B one or more selected from Mo: 0.50% or less, V: 0.50% or less, W: 0.50% or less, Co: 0.50% or less, B: 0.0100% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.
  • the texture has an X-ray intensity ratio of 0.90 or more for the (110) plane on the rolled surface at the 1/4 position of the sheet thickness
  • the high-strength extra thick steel plate according to [1] or [2] which has a steel structure at a 1/4 position in the plate thickness direction, which is a mixed structure consisting of, in terms of area fraction, 80 to 100% bainite phase and 0 to 20% ferrite phase, and in which the average grain size of bainite crystal grains surrounded by grain boundaries having an orientation difference of 15° or more is 20 ⁇ m or less.
  • the slab is hot-rolled under the conditions of a thickness of 350 mm or more and a reduction ratio, which represents the ratio of the slab thickness to the plate thickness of the final product, of 3.25 or more and less than 4.00.
  • cooling is performed under the conditions of a cooling start temperature at the 1/2 plate thickness position: Ar 3 point or higher, an average cooling rate in the temperature range of 700 to 500°C at the 1/2 plate thickness position: 2.0°C/s or higher, and a cooling stop temperature at the 1/2 plate thickness position: 500°C or lower.
  • the temperature at the 1/2 position of the plate thickness is the average reduction rate/pass in the austenite recrystallization temperature range: 3.5% or more;
  • a steel structure at the 1/2 position of the plate thickness is a mixed structure consisting of a bainite phase and a ferrite phase, the average grain size of the bainite crystal grains is 20 ⁇ m or less, and the circle equivalent diameter of the maximum porosity remaining in the center of the steel plate is 200 ⁇ m or less, so that a steel plate in which the porosity at the 1/2 position of the plate thickness is sufficiently compressed can be obtained.
  • the above-mentioned texture is present at the 1/2 position of the plate thickness, the linear progression of brittle cracks can be inhibited.
  • the high-strength extra-thick steel plate of the present invention has excellent toughness and brittle crack propagation arrest properties even when the plate thickness is over 100 mm. Furthermore, according to the manufacturing method of the present invention, a high-strength extra-thick steel plate having the above-mentioned properties can be manufactured by optimizing the rolling conditions.
  • the high-strength extra-thick steel plate of the present invention can be applied to deck members joined to hatch side coamings in the strong deck structures of container ships and bulk carriers, thereby contributing to improved ship safety.
  • the present invention is extremely useful industrially.
  • C 0.040 to 0.150%
  • C is an element that acts to increase the hardenability of steel and is necessary to achieve a desired strength.
  • the C content is set to 0.040% or more.
  • the C content is set to a range of 0.040 to 0.150%.
  • the preferred lower limit of the C content is 0.050% or more, more preferably 0.055% or more.
  • the preferred upper limit of the C content is 0.100% or less, more preferably 0.090% or less.
  • Si 0.02 to 0.50% Si is a component necessary for deoxidization. Si is also an element that has the effect of increasing the hardenability of steel by suppressing the generation of coarse carbides, and in order to achieve the desired strength, Si is contained at 0.02% or more. On the other hand, if the Si content exceeds 0.50%, not only the surface properties of the steel are impaired, but also the toughness is extremely deteriorated. For this reason, the Si content is set to a range of 0.02 to 0.50%.
  • the lower limit of the Si content is preferably 0.050% or more, and more preferably 0.10% or more.
  • the upper limit of the Si content is preferably 0.40% or less, and more preferably 0.30% or less.
  • Mn 1.00 to 2.50%
  • Mn is an element that has the effect of increasing the hardenability of steel, and is necessary to exhibit the desired strength.
  • the Mn content is set to 1.00% or more.
  • the Mn content is set to 2.50% or less.
  • the lower limit of the Mn content is preferably 1.50% or more, and more preferably 1.65% or more.
  • the upper limit of the Mn content is preferably 2.35% or less, and more preferably 2.15% or less.
  • P 0.020% or less
  • S 0.010% or less
  • P and S are inevitable impurities in steel. If their contents increase, toughness deteriorates.
  • the P content is suppressed to 0.020% or less and the S content is suppressed to 0.010% or less.
  • the P content is preferably 0.012% or less, and more preferably 0.006% or less.
  • the S content is preferably 0.006% or less, and more preferably 0.002% or less.
  • the lower limits of the P content and S content are not particularly limited. However, since excessive reduction of P and S leads to increased manufacturing costs, the P content and S content are preferably set to P: 0.0005% or more and S: 0.0005% or more, respectively. More preferably, P: 0.002% or more and S: 0.001% or more.
  • Al 0.010 to 0.100%
  • Al is an element that acts as a deoxidizer, and in order to obtain this effect, the Al content must be 0.010% or more.
  • the Al content is set to a range of 0.010 to 0.100%.
  • the lower limit of the Al content is preferably 0.020% or more, and more preferably 0.030% or more.
  • the upper limit of the Al content is preferably 0.070% or less, and more preferably 0.040% or less.
  • N 0.0010 to 0.0100% N combines with Al in the steel, adjusts the grain size during rolling, and strengthens the steel. To obtain this effect, the N content must be 0.0010% or more. If the N content exceeds 0.0100%, toughness deteriorates. For this reason, the N content is set to a range of 0.0010 to 0.0100%.
  • the lower limit of the N content is preferably 0.0020% or more, and more preferably 0.0025% or more.
  • the upper limit of the N content is preferably 0.0070% or less, and more preferably 0.0055% or less.
  • O 0.0100% or less
  • O oxygen
  • the O content is preferably 0.0050% or less, and more preferably 0.0030% or less.
  • the lower limit of the O content is not particularly limited and may be 0%.
  • O is an element that is inevitably contained in steel as an impurity, so industrially it may be more than 0%.
  • the O content is preferably 0.0009% or more, and more preferably 0.0020% or more.
  • each element is contained within the above range, and Ceq (carbon equivalent) (%) defined by formula (1) satisfies the following range.
  • Ceq C+Mn/6+Cu/15+Ni/15+Cr/5+Mo/5+V/5...
  • C, Mn, Cu, Ni, Cr, Mo and V in formula (1) represent the content (mass %) of each element, and the content of an element that is not contained is set to 0.
  • Ceq 0.480 to 0.560%
  • the value of Ceq represented by formula (1) is adjusted to 0.480% or more. This increases the hardenability of the steel plate, and even at the 1/2 plate thickness position where the cooling rate is the smallest, the steel structure becomes bainite throughout, thereby improving strength.
  • the value of Ceq exceeds 0.560%, the hardenability becomes excessive, the strength of the matrix structure increases excessively, and the amount of MA (martensite) generated, which is the brittle fracture origin, increases.
  • Ceq is set to 0.560% or less.
  • the value of Ceq is preferably set to 0.490% or more, more preferably set to 0.500% or more.
  • the value of Ceq is preferably set to 0.540% or less, more preferably set to 0.530% or less.
  • the above is the basic composition of the present invention, with the balance being Fe and unavoidable impurities.
  • the high strength extra thick steel plate of the present invention can obtain the desired properties.
  • each of the components Ti, Nb, Cu, Ni, Cr, Mo, V, W, Co, B, Ca, Mg, and REM can be contained as necessary, so these components may be 0%.
  • Ti: 0.030% or less Ti has the effect of forming nitrides, carbides, or carbonitrides by containing a small amount of Ti, refining the crystal grains, and improving the toughness of the base material. In order to obtain this effect, it is preferable to set the Ti content to 0.005% or more. On the other hand, if the Ti content exceeds 0.030%, the toughness of the base material and the welded heat affected zone may be reduced. Therefore, when Ti is contained, the Ti content is preferably 0.030% or less, and more preferably 0.025% or less. It is more preferable to set the Ti content to 0.010% or more.
  • Nb 0.050% or less Nb has the effect of increasing the hardenability of steel and expanding the non-recrystallization temperature range in rolling (hot rolling) in the austenite region. In order to obtain this effect, it is preferable to set the Nb content to 0.005% or more. On the other hand, if the Nb content exceeds 0.050%, coarse NbC may precipitate, which may lead to a decrease in toughness. Therefore, when Nb is contained, the Nb content is preferably 0.050% or less, and more preferably 0.040% or less. The Nb content is more preferably 0.010% or more.
  • Cu 2.00% or less
  • Cu is an element that enhances the hardenability of steel.
  • Cu directly contributes to improving the strength after rolling.
  • Cu can be contained to improve functions such as toughness, high-temperature strength, and weather resistance.
  • the Cu content is 0.01% or more.
  • the Cu content is preferably 2.00% or less, and more preferably 1.00% or less.
  • the Cu content is more preferably 0.05% or more, and even more preferably 0.10% or more.
  • Ni is an element that enhances the hardenability of steel. Ni directly contributes to improving the strength after rolling. In addition, Ni can be contained to improve functions such as toughness, high-temperature strength, and weather resistance. In order to obtain the above effects of this element, it is preferable that the Ni content is 0.01% or more. On the other hand, if the Ni content exceeds 2.50%, it will lead to deterioration of weldability and toughness and an increase in alloy cost. Therefore, when Ni is contained, it is preferable that the Ni content is 2.50% or less, and more preferably 2.00% or less. It is more preferable that the Ni content is 0.10% or more.
  • Cr is an element that enhances the hardenability of steel. Cr directly contributes to improving the strength after rolling. In addition, Cr can be contained to improve functions such as toughness, high-temperature strength, and weather resistance. In order to obtain the above effects of this element, the Cr content is preferably 0.01% or more. On the other hand, if the Cr content exceeds 2.00%, it will lead to deterioration of weldability and toughness and an increase in alloy cost. Therefore, when Cr is contained, the Cr content is preferably 2.00% or less, and more preferably 1.00% or less. The Cr content is more preferably 0.05% or more, and even more preferably 0.10% or more.
  • Group B One or more selected from Mo: 0.50% or less, V: 0.50% or less, W: 0.50% or less, Co: 0.50% or less, B: 0.0100% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less Mo: 0.50% or less Mo is an element that enhances the hardenability of steel. Mo directly contributes to improving the strength after rolling. In addition, Mo can be contained to improve functions such as toughness, high-temperature strength, and weather resistance. In order to obtain the above effects of this element, it is preferable to set the Mo content to 0.01% or more.
  • the Mo content exceeds 0.50%, it will cause deterioration of weldability and toughness and an increase in alloy cost. Therefore, when Mo is contained, it is preferable to set the Mo content to 0.50% or less, and more preferably to 0.30% or less.
  • the Mo content is more preferably 0.03% or more.
  • V 0.50% or less
  • V is an element that improves the strength of steel by precipitation strengthening, which is precipitated as V(CN). This effect is exhibited by making the V content 0.001% or more. However, if the V content exceeds 0.50%, the toughness may decrease. Therefore, when V is contained, the V content is preferably 0.50% or less, and more preferably 0.30% or less. The V content is more preferably 0.005% or more, and even more preferably 0.010% or more.
  • W 0.50% or less W is an element that has the effect of improving the strength of the steel plate.
  • the W content is preferably 0.001% or more.
  • the W content is preferably 0.50% or less, and more preferably 0.30% or less.
  • the W content is more preferably 0.005% or more.
  • Co 0.50% or less
  • Co is an element that has the effect of improving the strength of the steel plate.
  • the Co content is preferably 0.001% or more.
  • the Co content is preferably 0.50% or less, more preferably 0.40% or less, and even more preferably 0.30% or less.
  • the Co content is more preferably 0.005% or more.
  • B 0.0100% or less
  • B is an element that enhances the hardenability of steel in small amounts. However, if the content of B exceeds 0.0100%, the toughness of the welded part is reduced. Therefore, when B is contained, the B content is preferably 0.0100% or less, and more preferably 0.0030% or less. In order to improve the strength of the steel plate, the B content is preferably 0.0001% or more, more preferably 0.0005% or more, and even more preferably 0.0010% or more.
  • Ca 0.0100% or less Ca refines the structure of the weld heat affected zone and improves toughness.
  • the Ca content is preferably 0.0005% or more, more preferably 0.0020% or more.
  • the Ca content exceeds 0.0100%, coarse inclusions are formed, which deteriorates toughness. Therefore, when Ca is contained, the Ca content is preferably 0.0100% or less, more preferably 0.050% or less.
  • Mg 0.0100% or less Like Ca, Mg refines the structure of the welded heat affected zone and improves toughness. In order to obtain this effect, when Mg is contained, the Mg content is preferably 0.0005% or more, and more preferably 0.0020% or more. On the other hand, when the Mg content exceeds 0.0100%, coarse inclusions are formed, which deteriorates toughness. Therefore, when Mg is contained, the Mg content is preferably 0.0100% or less, and more preferably 0.0050% or less.
  • REM 0.0200% or less
  • the REM content is preferably 0.0005% or more, more preferably 0.0015% or more, and even more preferably 0.0100% or more.
  • the REM content is preferably 0.0200% or less.
  • the X-ray intensity ratio of the (211) plane on the rolled surface at the 1/2 position of the plate thickness 1.60 or more. If the X-ray intensity ratio of the (211) plane is less than 1.60, the brittle crack is likely to progress linearly, and as a result, the brittle crack propagation arrestability of the plate thickness is reduced.
  • the X-ray intensity ratio of the (211) plane on the rolled surface at the 1/2 position of the plate thickness is made 1.60 or more.
  • the X-ray intensity ratio of the (211) plane is preferably 1.70 or more, more preferably 1.80 or more.
  • the X-ray intensity ratio of the (211) plane is preferably 2.50 or less, and more preferably 2.30 or less.
  • the X-ray intensity ratio of the (211) plane is a value that represents the degree of integration of the (211) crystal plane of the target material (i.e., high-strength extra-thick steel plate).
  • the X-ray intensity ratio of the (211) plane is calculated as the ratio (i.e., I(211)/I0 (211) ) of the X-ray diffraction intensity of the (211) reflection of the target material (I ( 211 )) to the X-ray diffraction intensity of the (211) reflection of a random standard sample without texture, as described in the Examples below.
  • the steel structure at the 1/2 plate thickness position is a mixed structure consisting of, in terms of area fraction, 80 to 100% bainite phase and 0 to 20% ferrite phase, the average grain size of bainite crystal grains surrounded by grain boundaries with an orientation difference of 15° or more is 20 ⁇ m or less, and the circle equivalent diameter of the maximum porosity remaining at the 1/2 plate thickness position (plate thickness center portion) is 200 ⁇ m or less.
  • the area fraction of the bainite phase at the 1/2 plate thickness position must be 80 to 100%. If the area fraction of the bainite phase is less than 80%, the fraction of hard structures decreases and the texture of the (211) plane does not develop sufficiently, resulting in a decrease in strength and brittle crack propagation arrestability. Therefore, the area fraction of the bainite phase at the 1/2 plate thickness position is set to 80% or more. In order to further increase the strength and brittle crack propagation arrestability, the above-mentioned area fraction is preferably 85% or more, and more preferably 90% or more.
  • the high-strength extra-thick steel plate of the present invention needs to have an area fraction of ferrite phase at 1/2 thickness position of 0 to 20%. If the area fraction of ferrite phase exceeds 20%, the fraction of hard structure decreases and the texture of the (211) plane does not develop sufficiently, resulting in a decrease in strength and brittle crack propagation arrestability. Therefore, the area fraction of ferrite phase at 1/2 thickness position is set to 20% or less. In order to further increase the strength and brittle crack propagation arrestability, the above area fraction is preferably set to 15% or less, more preferably 10% or less.
  • the average grain size of bainite grains at the 1/2 position of the plate thickness must be 20 ⁇ m or less. If this average grain size exceeds 20 ⁇ m, the grain size becomes coarse and the fracture surface unit of the cleavage fracture surface of the grain becomes large, so that the toughness and brittle crack propagation arrestability are reduced. Therefore, the average grain size at the 1/2 position of the plate thickness is set to 20 ⁇ m or less. In order to further improve the toughness and brittle crack propagation arrestability, the above average grain size is preferably 19 ⁇ m or less, and more preferably 18 ⁇ m or less. The lower limit of the average grain size is not particularly specified. From the viewpoint of rolling efficiency, the average grain size is preferably 5 ⁇ m or more, and more preferably 10 ⁇ m or more.
  • the circle-equivalent diameter of the maximum porosity remaining at the 1/2 position of the plate thickness must be 200 ⁇ m or less. If the circle-equivalent diameter of the maximum porosity exceeds 200 ⁇ m, the porosity becomes the fracture origin and the toughness significantly decreases. Therefore, the circle-equivalent diameter of the maximum porosity remaining at the 1/2 position of the plate thickness is set to 200 ⁇ m or less. In order to further increase the toughness, the circle-equivalent diameter is preferably set to 150 ⁇ m or less, and more preferably set to 100 ⁇ m or less.
  • the lower limit of the circle-equivalent diameter is not particularly specified. From the viewpoint of rolling efficiency, the circle-equivalent diameter is preferably set to 25 ⁇ m or more, more preferably set to 50 ⁇ m or more, and even more preferably set to 70 ⁇ m or more.
  • the present invention may also have the configurations described below.
  • the steel structure at the 1/4 position of the plate thickness is preferably a mixed structure consisting of 80 to 100% bainite phase and 0 to 20% ferrite phase in terms of area fraction, and the average grain size of bainite crystal grains surrounded by grain boundaries with an orientation difference of 15° or more is preferably 20 ⁇ m or less.
  • the area fraction of the bainite phase at the 1/4 position of the plate thickness is preferably 80 to 100%. If the area fraction of the bainite phase is less than 80%, the fraction of hard structures is reduced and the texture of the (110) plane is not sufficiently developed, resulting in reduced strength and brittle crack propagation arrestability. Therefore, it is desirable that the area fraction of the bainite phase at the 1/4 position of the plate thickness is 80% or more. In order to further increase the strength and brittle crack propagation arrestability, the above-mentioned area fraction is preferably 85% or more, and more preferably 90% or more.
  • the area fraction of the ferrite phase at the 1/4 position of the plate thickness is preferably 0 to 20%. If the area fraction of the ferrite phase exceeds 20%, the fraction of hard structures is reduced and the texture of the (110) plane is not sufficiently developed, so that the strength and brittle crack propagation arrestability are reduced. Therefore, it is preferable that the area fraction of the ferrite phase at the 1/4 position of the plate thickness is 20% or less. In order to further increase the strength and brittle crack propagation arrestability, the above-mentioned area fraction is preferably 15% or less, and more preferably 10% or less.
  • the average grain size of bainite grains at the 1/4 position of the plate thickness is preferably 20 ⁇ m or less. If this average grain size exceeds 20 ⁇ m, the fracture surface unit of the cleavage fracture surface of the grains becomes larger due to the grain size coarsening, and the brittle crack propagation arrestability decreases. Therefore, it is preferable that the average grain size of bainite grains at the 1/4 position of the plate thickness is 20 ⁇ m or less. In order to further improve the brittle crack propagation arrestability, the above average grain size is preferably 19 ⁇ m or less, and more preferably 16 ⁇ m or less.
  • the average grain size is preferably 5 ⁇ m or more, and more preferably 10 ⁇ m or more.
  • ⁇ Texture> (optimal conditions) [X-ray intensity ratio of the (110) plane on the rolled surface at the 1/4 position of the plate thickness: 0.90 or more]
  • the X-ray intensity ratio of the (110) plane on the rolled surface at the 1/4 position of the plate thickness is set to 0.90 or more.
  • the X-ray intensity ratio of the (110) plane is preferably 1.00 or more, more preferably 1.10 or more.
  • the X-ray intensity ratio of the (110) plane is preferably 1.50 or less, and more preferably 1.30 or less.
  • the X-ray intensity ratio of the (110) plane is a value that represents the degree of integration of the (110) crystal plane of the target material (high-strength extra-thick steel plate).
  • the X-ray intensity ratio of the (110) plane is calculated as the ratio (i.e., I(110)/I0 (110) ) of the X-ray diffraction intensity of the (110) reflection of the target material (I ( 110 ) ) to the X-ray diffraction intensity of the ( 110) reflection of a random standard sample without texture, as described in the Examples below.
  • the high-strength extra thick steel plate of the present invention has a yield strength of 390 MPa or more, measured using a ⁇ 14 mm JIS 14A tensile test piece taken from a depth of 1/2 the plate thickness (i.e., at the 1/2 plate thickness position).
  • Ships such as container ships and bulk carriers normally use high-strength, thick steel plate base material that can withstand this bending stress, and a yield strength of less than 390 MPa is not suitable for use.
  • vTrs If the transition temperature is higher than -100°C, the brittle crack propagation arrestability of the plate thickness decreases. Therefore, the high-strength extra-thick steel plate of the present invention has a vTrs at 1/2 thickness position of -100°C or less.
  • the vTrs In order to further improve the brittle crack propagation arrestability, it is preferable to set the vTrs at -110°C or less, and more preferably to set the vTrs at -120°C or less.
  • the lower limit of vTrs is not particularly specified. From the viewpoint of rolling efficiency, the vTrs is preferably -160°C or more, and more preferably -150°C or more.
  • vTrs can be evaluated by taking a JIS No. 4 impact test specimen from the 1/2 position of the plate thickness of a high-strength extra-thick steel plate and conducting a Charpy test, as described in the examples below.
  • Kca (-10°C) value 8400 N/mm3 /2 or more Extra thick steel plates with a plate thickness of more than 100 mm need to have a Kca (-10°C) value of 8400 N/mm3 /2 or more to prevent brittle crack propagation in the hull.
  • Kca (-10°C) value 8400 N/mm3 /2 or more
  • the Kca value at -10°C is preferably 25000 N/mm3 /2 or less, and more preferably 20000 N/mm3 /2 or less.
  • the Kca value can be evaluated using a standard temperature gradient ESSO test, as described in the examples below.
  • the high-strength extra-thick steel plate of the present invention has high strength, high toughness, and high (excellent) brittle crack propagation arrestability, even with a plate thickness of more than 100 mm.
  • the thickness of the high-strength extra-thick steel plate of the present invention there is no particular upper limit to the thickness of the high-strength extra-thick steel plate of the present invention. From the viewpoint of rolling efficiency, it is preferable that the upper limit of the plate thickness be 180 mm or less.
  • the high-strength extra-thick steel plate of the present invention is manufactured by subjecting a steel material having the above-mentioned composition to a heating process, a hot rolling process, and a cooling process under the specific conditions described below.
  • the temperature in each process refers to the temperature at the center of the plate thickness (i.e., 1/2 the plate thickness position) of the steel material and hot-rolled plate. For example, it can be determined by calculating the temperature distribution in the cross section of the steel plate using heat transfer analysis and correcting the result by the surface temperature of the steel plate.
  • Heating temperature of steel material 1000-1200°C
  • the heating temperature is set to 1000°C or higher.
  • the heating temperature of the steel material is high and exceeds 1200°C, the austenite grains become coarse, resulting in a decrease in toughness and a failure to obtain the desired brittle crack propagation arrest characteristic.
  • the strength of the steel plate decreases.
  • oxidation becomes severe, oxidation loss increases, and there is a risk of a decrease in yield.
  • the heating temperature is set to 1200°C or lower.
  • the heating temperature is preferably 1050°C or higher, more preferably 1080°C or higher.
  • the heating temperature is preferably 1150°C or lower, more preferably 1130°C or lower.
  • ⁇ Hot rolling process> the steel material heated in the heating process is subjected to hot rolling under the following conditions: a rolling start temperature at the 1/2 thickness position: ( Ar3 point + 100)°C or higher; a cumulative reduction rate in the austenite recrystallization temperature range at the 1/2 thickness position: 5.0% or higher; a cumulative reduction rate in the austenite non-recrystallization temperature range at the 1/2 thickness position: 50.0% or higher; and a rolling end temperature at the 1/2 thickness position: Ar3 point or higher; a slab thickness of 350 mm or more; and a reduction ratio, which represents the ratio of the slab thickness to the plate thickness of the final product, of 3.25 or more and less than 4.00.
  • Rolling start temperature ( Ar3 point + 100) ° C. or higher]
  • the rolling start temperature is preferably set to ( Ar3 point + 150) ° C. or higher, and more preferably set to ( Ar3 point + 200) ° C. or higher.
  • the upper limit of the rolling start temperature may be in accordance with the heating temperature of the steel material described above. That is, the rolling start temperature is preferably set to 1150 ° C. or lower, and more preferably set to 1130 ° C. or lower.
  • the Ar3 point ( Ar3 transformation point) (°C) can be calculated according to the following formula (3).
  • Ar 3 point (°C) 910 - 273 x C - 74 x Mn - 57 x Ni - 16 x Cr - 9 x Mo - 5 x Cu ...
  • each element symbol represents the content (mass%) of the corresponding element in the steel, and elements that are not contained are represented as 0.
  • the cumulative reduction in this temperature range is preferably 10% or more, and more preferably 15% or more.
  • the upper limit of the cumulative rolling reduction in this temperature range is not particularly limited. Since the effect of improving the grain refinement is saturated, the cumulative rolling reduction in this temperature range is preferably 45% or less, and more preferably 40% or less.
  • the cumulative reduction in the austenite recrystallization temperature range be 5.0% or more in the temperature range of 1100 to 950°C.
  • the cumulative reduction rate in this temperature range is less than 50%, the austenite does not elongate sufficiently in the rolling direction, reducing the number of nucleation sites during bainite transformation, which results in the formation of coarse bainite and makes it impossible to refine the grain size.
  • the Charpy fracture transition temperature (vTrs) at the 1/2 position in the plate thickness: -100°C or less is not achieved.
  • a texture with a (211) plane concentration of 1.60 or more on the rolled surface in the plate thickness center cannot be obtained.
  • the cumulative rolling reduction in this temperature range is set to 50.0% or more.
  • the cumulative rolling reduction is preferably 55% or more, and more preferably 60% or more.
  • the cumulative reduction rate in this temperature range there is no particular upper limit to the cumulative reduction rate in this temperature range. From the viewpoint of not impeding the rolling efficiency, it is preferable that the cumulative reduction rate in this temperature range be 75% or less, and more preferably 70% or less.
  • the cumulative reduction in the austenite non-recrystallization temperature range is preferably 50.0% or more in the temperature range of less than 950°C and 700°C or more.
  • the hot rolling process must be completed at a rolling end temperature at the 1/2 plate thickness position of Ar3 point (°C) or higher. If the temperature of the steel plate during hot rolling is lower than Ar3 point (°C), phase transformation to ferrite begins, and the fraction of bainite that increases the X-ray intensity of the (211) plane decreases, so the X-ray intensity ratio of the (211) plane decreases. As a result, excellent brittle crack propagation arrest properties cannot be obtained. Furthermore, the lower the temperature, the higher the deformation resistance, which causes a problem of increased load on the hot rolling machine.
  • the rolling end temperature is preferably ( Ar3 point + 10) °C or higher from the viewpoint of setting the cooling start temperature of the subsequent process to Ar3 point (°C) or higher.
  • the rolling end temperature is preferably ( Ar3 point + 60)°C or less, and more preferably ( Ar3 point + 50)°C or less.
  • the thickness of the hot-rolled sheet after the hot rolling process is as follows: Specifically, the thickness of the slab is 350 mm or more, and the rolling in the hot rolling process is controlled so that the ratio of the slab thickness to the sheet thickness of the final product (rolling reduction ratio) is 3.25 or more.
  • the reduction ratio is less than 3.25, the steel structure is not sufficiently refined, and toughness is not improved. As a result, the Charpy fracture transition temperature at 1/2 the plate thickness: -100°C or less is not achieved. Furthermore, if the reduction ratio is less than 3.25, the rolling stress applied to the 1/2 plate thickness position is insufficient, and deformation does not progress in the direction in which the porosity generated inside the steel plate closes, and even when rolling is completed, coarse porosity remains and becomes the starting point of fracture. As a result, the porosity generated inside the steel plate does not bond, and toughness is significantly reduced.
  • the reduction ratio is preferably 3.40 or more, and more preferably 3.50 or more.
  • the reduction ratio must be less than 4.00.
  • the reduction ratio is preferably 3.80 or less, and more preferably 3.70 or less.
  • the above-mentioned effects can be obtained by performing hot rolling under the above-mentioned hot rolling conditions. From the viewpoint of obtaining the effects more effectively, it is also effective to further specify the following hot rolling conditions. Specifically, the temperature at the 1/2 thickness position is set to an average reduction rate/pass of 3.5% or more in the austenite recrystallization temperature range, and the rolling end temperature at the 1/4 thickness position is set to Ar 3 point °C or more.
  • the average rolling reduction/pass in this temperature range there is no particular upper limit to the average rolling reduction/pass in this temperature range. From the viewpoint of production load, it is preferable that the average rolling reduction/pass in this temperature range be 10% or less, and more preferably 8.0% or less.
  • the upper limit of the rolling end temperature is not particularly limited. From the viewpoint of rolling efficiency, the rolling end temperature is preferably ( Ar3 point + 50) ° C. or less, and more preferably ( Ar3 point + 40) ° C. or less.
  • the hot-rolled sheet hot-rolled in the hot rolling process is cooled under the following conditions: a cooling start temperature at 1/2 thickness position: Ar 3 point or higher, an average cooling rate in the temperature range of 700 to 500°C at the 1/2 thickness position: 2.0°C/s or higher, and a cooling stop temperature at the 1/2 thickness position: 500°C or lower.
  • the cooling start temperature is set to be Ar3 point (°C) or higher.
  • the cooling start temperature is preferably set to be ( Ar3 point + 10) °C or higher, and is preferably set to be ( Ar3 point + 40) °C or lower.
  • the temperature range for measuring this average cooling rate is set to 700 to 500°C, from the viewpoint of obtaining the effect in which most of the austenite structure transforms and contributes greatly to the properties of the steel plate.
  • the average cooling rate in the temperature range of 700 to 500°C at the 1/2 plate thickness position is set to 2.0°C/s or more. This has the effect of increasing the proportion of bainite, improving strength, and developing the texture of the (211) plane, improving brittle crack propagation arrest properties.
  • the average cooling rate in this temperature range is preferably 3.0°C/s or more.
  • the upper limit of the average cooling rate is not particularly limited. From the viewpoint of avoiding an increase in cooling costs due to excessive rapid cooling, the average cooling rate is preferably 20°C/s or less, and more preferably 10°C/s or less.
  • Average cooling rates outside the above temperature range of 700 to 500°C are not specified because they do not have a significant effect on bainite formation. From the standpoint of manufacturing efficiency, it is preferable to set the rate at 0.5 to 0.1°C/s.
  • the cooling process needs to be performed until the temperature at the 1/2 position of the plate thickness is 500°C or less. In other words, it needs to be performed until the cooling stop temperature is 500°C or less. If the cooling stop temperature exceeds 500°C, a large amount of ferrite is generated in the steel, so that the area fraction of bainite cannot be increased. As a result, the X-ray intensity ratio of the (211) plane decreases, and excellent brittle crack propagation stopping properties cannot be obtained. In addition, the strength decreases.
  • the cooling stop temperature is preferably 450°C or less, more preferably 400°C or less.
  • the cooling stop temperature is preferably 200°C or more, more preferably 300°C or more.
  • Table 1 shows the chemical composition of the test steels
  • Table 2 shows the manufacturing conditions. Molten steels (steel symbols: A to AG) with the chemical compositions shown in Table 1 were melted in a converter and made into steel material using a continuous casting method. The heating process, hot rolling process, and cooling process were then carried out in that order under the manufacturing conditions shown in Table 2, to produce high-strength extra thick steel plates (steel symbols: 1 to 42) with the plate thicknesses shown in Table 3. Note that blank spaces in Table 1 indicate that an element was not intentionally added, and include not only cases where an element is not contained (i.e. 0%), but also cases where an element is unavoidably contained.
  • the texture was evaluated by measuring the X-ray intensity ratio of the (211) plane at the 1/2 position of the sheet thickness of the steel sheet. From the obtained high-strength extra-thick steel plate, a plate-shaped sample having dimensions of 1 mm in thickness with the plate thickness 1/2 position as the plate thickness center, 22 mm in the direction parallel to the rolling direction, and 25 mm in the direction perpendicular to the rolling direction was taken, and a surface parallel to the surface of the sample was mechanically polished and electrolytically polished to prepare a test piece for X-ray diffraction. Using this test piece, X-ray diffraction measurement was performed using an X-ray diffractometer using a Mo radiation source, and the X-ray intensity ratio of the (211) plane was obtained.
  • the X-ray intensity ratio of the (110) plane at a position corresponding to 1/4 of the sheet thickness of the steel sheet was measured. From the obtained high-strength extra-thick steel plate, a plate-shaped sample having dimensions of 1 mm in thickness with the 1/4 position at the plate thickness center, 22 mm in the direction parallel to the rolling direction, and 25 mm in the direction perpendicular to the rolling direction was taken, and a surface parallel to the surface of the sample was mechanically polished and electrolytically polished to prepare a test piece for X-ray diffraction. Using this test piece, X-ray diffraction measurement was performed using an X-ray diffractometer using a Mo radiation source, and the X-ray intensity ratio of the (110) plane was obtained.
  • the steel structure at the 1/2 sheet thickness position was measured as follows. A sample was taken from the width center of the steel plate at 1/2 the plate thickness so that the surface perpendicular to the rolling direction was the observation surface. The dimensions of the sample were 20 mm in the plate thickness direction, 10 mm in the direction parallel to the rolling direction, and 1 mm in the direction perpendicular to the rolling direction. The surface perpendicular to the rolling direction of this sample was mirror-polished, and then an optical microscope photograph of the metal structure revealed by nital etching was taken. The photographed portion was at 1/2 the plate thickness position, and the magnification was 200 times. The area fractions of the bainite phase and ferrite phase were evaluated by calculating the area fractions by image analysis, assuming that the structure revealed as white chunks in the obtained photograph was ferrite and the remaining part was bainite.
  • the steel structure at the 1/4 position of the plate thickness was measured as follows. A sample was taken from the center of the width of the steel plate, at 1/4 of the plate thickness, so that the surface perpendicular to the rolling direction was the observation surface. The dimensions of the sample were 20 mm in the plate thickness direction, 10 mm in the direction parallel to the rolling direction, and 1 mm in the direction perpendicular to the rolling direction. After mirror polishing the surface perpendicular to the rolling direction of this sample, an optical microscope photograph of the metal structure revealed by nital etching was taken. The photographed area was at 1/4 of the plate thickness position, and the magnification was 200 times. The area fractions of the bainite phase and ferrite phase were evaluated by image analysis of the obtained photograph.
  • the average grain size of bainite grains at the 1/2 position of the sheet thickness was measured as follows. A sample was taken from the center of the width of the steel plate, at 1/2 the plate thickness, so that the surface perpendicular to the rolling direction was the observation surface. The dimensions of the sample were 20 mm in the plate thickness direction, 10 mm in the direction parallel to the rolling direction, and 1 mm in the direction perpendicular to the rolling direction. After mirror polishing the surface perpendicular to the rolling direction of this sample, EBSP analysis was performed at the 1/2 plate thickness position under the following conditions.
  • the circle equivalent diameter of the structure surrounded by high-angle grain boundaries with an orientation difference of 15° or more with adjacent crystal grains was obtained, and the average value of the circle equivalent diameter in the following analysis region was taken as the average effective crystal grain size.
  • the average grain size of bainite grains at the 1/4 position of the plate thickness was measured as follows. A sample was taken from the center of the width of the steel plate, at 1/4 of the plate thickness, so that the surface perpendicular to the rolling direction was the observation surface.
  • the dimensions of the sample were 20 mm in the plate thickness direction, 10 mm in the direction parallel to the rolling direction, and 1 mm in the direction perpendicular to the rolling direction.
  • EBSP analysis was performed at the 1/4 plate thickness position under the following conditions. From the obtained crystal orientation map, the circle equivalent diameter of the structure surrounded by high-angle grain boundaries with an orientation difference of 15° or more with adjacent crystal grains was obtained, and the average value of the circle equivalent diameter in the following analysis region was taken as the average effective crystal grain size.
  • the brittle crack propagation arrest property was evaluated by determining the Kca value.
  • a temperature gradient type standard ESSO test was carried out to determine the Kca value at -10°C (Kca (-10°C) value (N/mm 3/2 )).
  • Kca (-10°C) value (N/mm 3/2 )
  • Three specimens were taken from each of the obtained high-strength extra-thick steel plates.
  • the size of the specimen was total thickness x L: 500 x W: 500 (mm).
  • the Kca value was calculated from the results of the three-body test. In this case, a value of Kca (-10°C) of 8400 N/mm 3/2 or more was evaluated as having excellent brittle crack propagation arrest properties.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Physics & Mathematics (AREA)
  • Thermal Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Heat Treatment Of Steel (AREA)
PCT/JP2023/031503 2022-11-14 2023-08-30 高強度極厚鋼板およびその製造方法 Ceased WO2024105967A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2023573540A JP7468814B1 (ja) 2022-11-14 2023-08-30 高強度極厚鋼板およびその製造方法
CN202380059615.9A CN119630827A (zh) 2022-11-14 2023-08-30 高强度极厚钢板及其制造方法
KR1020257004200A KR20250034987A (ko) 2022-11-14 2023-08-30 고강도 극후 강판 및 그의 제조 방법

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-181478 2022-11-14
JP2022181478 2022-11-14

Publications (1)

Publication Number Publication Date
WO2024105967A1 true WO2024105967A1 (ja) 2024-05-23

Family

ID=91084347

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/031503 Ceased WO2024105967A1 (ja) 2022-11-14 2023-08-30 高強度極厚鋼板およびその製造方法

Country Status (4)

Country Link
JP (1) JP7468814B1 (cg-RX-API-DMAC7.html)
KR (1) KR20250034987A (cg-RX-API-DMAC7.html)
CN (1) CN119630827A (cg-RX-API-DMAC7.html)
WO (1) WO2024105967A1 (cg-RX-API-DMAC7.html)

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2017047088A1 (ja) * 2015-09-18 2017-03-23 Jfeスチール株式会社 構造用高強度厚鋼板およびその製造方法
JP2017186614A (ja) * 2016-04-06 2017-10-12 新日鐵住金株式会社 厚鋼板およびその製造方法
WO2020262638A1 (ja) * 2019-06-27 2020-12-30 日本製鉄株式会社 鋼材及びその製造方法
WO2022097589A1 (ja) * 2020-11-05 2022-05-12 Jfeスチール株式会社 鋼板およびその製造方法
KR20230094389A (ko) * 2021-12-21 2023-06-28 주식회사 포스코 강도 및 저온 충격인성이 우수한 플랜지용 극후물 강재 및 그 제조방법

Family Cites Families (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP4077167B2 (ja) 2001-02-28 2008-04-16 株式会社神戸製鋼所 アレスト特性に優れた鋼板およびその製法
JP5064149B2 (ja) 2006-12-14 2012-10-31 新日本製鐵株式会社 脆性き裂伝播停止性能に優れた高強度厚鋼板及びその製造方法
CN102666884B (zh) 2010-02-08 2013-07-31 新日铁住金株式会社 厚钢板的制造方法
JP5759109B2 (ja) 2010-03-09 2015-08-05 株式会社神戸製鋼所 脆性亀裂伝播停止特性に優れた鋼材、およびその製造方法
JP5522084B2 (ja) 2011-02-24 2014-06-18 新日鐵住金株式会社 厚鋼板の製造方法

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2017047088A1 (ja) * 2015-09-18 2017-03-23 Jfeスチール株式会社 構造用高強度厚鋼板およびその製造方法
JP2017186614A (ja) * 2016-04-06 2017-10-12 新日鐵住金株式会社 厚鋼板およびその製造方法
WO2020262638A1 (ja) * 2019-06-27 2020-12-30 日本製鉄株式会社 鋼材及びその製造方法
WO2022097589A1 (ja) * 2020-11-05 2022-05-12 Jfeスチール株式会社 鋼板およびその製造方法
KR20230094389A (ko) * 2021-12-21 2023-06-28 주식회사 포스코 강도 및 저온 충격인성이 우수한 플랜지용 극후물 강재 및 그 제조방법

Also Published As

Publication number Publication date
JP7468814B1 (ja) 2024-04-16
KR20250034987A (ko) 2025-03-11
CN119630827A (zh) 2025-03-14
JPWO2024105967A1 (cg-RX-API-DMAC7.html) 2024-05-23

Similar Documents

Publication Publication Date Title
KR101642196B1 (ko) 강판
KR101681491B1 (ko) 취성 균열 전파 정지 특성이 우수한 고강도 후강판
JP6536514B2 (ja) 脆性亀裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法
JP5434145B2 (ja) 脆性亀裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法
KR101984531B1 (ko) 취성 균열 전파 정지 특성과 대입열 용접 특성이 우수한 대입열 용접용 고강도 강판과 그의 제조 방법
JP7099653B1 (ja) 鋼板およびその製造方法
WO2020153085A1 (ja) 厚鋼板およびその製造方法
JP5812193B2 (ja) 脆性き裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法
JP5035199B2 (ja) 脆性亀裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法
JP7396512B2 (ja) 厚鋼板および厚鋼板の製造方法
JP2008214653A (ja) 脆性亀裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法
JP7508029B1 (ja) 高強度極厚鋼板およびその製造方法
KR20190035875A (ko) 고강도 후강판 및 그의 제조 방법
JP7323090B1 (ja) 鋼板および鋼板の製造方法
JP7468814B1 (ja) 高強度極厚鋼板およびその製造方法
JP7127752B2 (ja) 鋼板およびその製造方法
KR102192969B1 (ko) 취성 균열 전파 정지 특성이 우수한 고강도 극후강판 및 그 제조 방법
WO2023149157A1 (ja) 鋼板およびその製造方法
JP5838801B2 (ja) 厚鋼板及び厚鋼板の製造方法
JP7396322B2 (ja) 鋼板
JP6504131B2 (ja) 高強度厚鋼板およびその製造方法
JP2025178632A (ja) 鋼板およびその製造方法
WO2025079722A1 (ja) 鋼材及び圧力容器
WO2025022587A1 (ja) 鋼板およびその製造方法
JP2026001684A (ja) 鋼板およびその製造方法

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 2023573540

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23891126

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 20257004200

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020257004200

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 202380059615.9

Country of ref document: CN

WWP Wipo information: published in national office

Ref document number: 1020257004200

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 202380059615.9

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 23891126

Country of ref document: EP

Kind code of ref document: A1