WO2023145965A1 - 結晶化された無機組成物物品 - Google Patents
結晶化された無機組成物物品 Download PDFInfo
- Publication number
- WO2023145965A1 WO2023145965A1 PCT/JP2023/003045 JP2023003045W WO2023145965A1 WO 2023145965 A1 WO2023145965 A1 WO 2023145965A1 JP 2023003045 W JP2023003045 W JP 2023003045W WO 2023145965 A1 WO2023145965 A1 WO 2023145965A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- component
- content
- less
- glass
- inorganic composition
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C03—GLASS; MINERAL OR SLAG WOOL
- C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03C3/00—Glass compositions
- C03C3/04—Glass compositions containing silica
- C03C3/076—Glass compositions containing silica with 40% to 90% silica, by weight
- C03C3/097—Glass compositions containing silica with 40% to 90% silica, by weight containing phosphorus, niobium or tantalum
-
- C—CHEMISTRY; METALLURGY
- C03—GLASS; MINERAL OR SLAG WOOL
- C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03C10/00—Devitrified glass ceramics, i.e. glass ceramics having a crystalline phase dispersed in a glassy phase and constituting at least 50% by weight of the total composition
- C03C10/0018—Devitrified glass ceramics, i.e. glass ceramics having a crystalline phase dispersed in a glassy phase and constituting at least 50% by weight of the total composition containing SiO2, Al2O3 and monovalent metal oxide as main constituents
- C03C10/0027—Devitrified glass ceramics, i.e. glass ceramics having a crystalline phase dispersed in a glassy phase and constituting at least 50% by weight of the total composition containing SiO2, Al2O3 and monovalent metal oxide as main constituents containing SiO2, Al2O3, Li2O as main constituents
-
- C—CHEMISTRY; METALLURGY
- C03—GLASS; MINERAL OR SLAG WOOL
- C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03C2204/00—Glasses, glazes or enamels with special properties
Definitions
- the present invention relates to a crystallized inorganic composition article.
- Crystallized glass is an example of glass with increased strength. Crystallized glass is obtained by depositing crystals inside the glass, and is known to be superior in mechanical strength to amorphous glass.
- Patent Document 1 discloses a glass-ceramic material having a transparent or translucent petalite crystalline phase and a lithium silicate crystalline phase with rapid ion exchangeability and high fracture toughness.
- Patent Document 2 discloses glass-ceramics for optical filters that have a good coefficient of thermal expansion and good light transmittance at the operating temperature, since the substrate material during film formation is about 200°C.
- Patent Document 3 discloses glass-ceramics for optical filters that have a good thermal expansion coefficient and light transmittance at the operating temperature during film formation.
- Patent Document 4 discloses a thermal recording medium that has good surface properties that can be sufficiently applied to the ramp load system for high-density recording, has high strength that can withstand high-speed rotation and drop impact, and is suitable for each drive member.
- an inorganic composition article for disc substrates for information recording media which has both expansion properties and heat resistance, a low melting temperature, and high productivity.
- the object of the present invention is to obtain a curved surface shape by heat processing, which has high mechanical strength that can be used for the cover glass of smartphones and the glass member of the housing, and excellent transparency even after heat processing.
- An object of the present invention is to provide an inorganic composition article.
- the present invention provides the following.
- (Configuration 1) An inorganic composition article characterized by having a transmittance of 50% or more at 550 nm when heated to [At + 50] ° C., where At (° C.) is the yield point,
- the raw glass is the mass % of oxide conversion, SiO 2 component content 65.0% to 85.0%, Al 2 O 3 component content 3.0% to 15.0%, Content of P 2 O 5 components: more than 0% to 5.0%, Li 2 O component content more than 5.0% to 15.0%, ZrO 2 component content 0% to 10.0%, Content of MgO component 0% to 5.0%, [Content of Al 2 O 3 components/(Content of K 2 O component + Content of MgO component)] >0 to 20.0, [Li 2 O component content/MgO component content] 8.0 or more,
- a crystallized inorganic composition article that is (Configuration 2) % by mass of the raw glass in terms of oxide, Content of K 2 O component 0% to 5.0%, Content of Zn
- a crystallized inorganic composition article comprising one or more crystalline phases selected from lithium disilicate, petalite, vergilite, beta-quartz and lithium monosilicate.
- Composition 4 % by mass of the raw glass in terms of oxide, Total content of Li 2 O component, Na 2 O component and K 2 O component [content of Li 2 O + content of Na 2 O component + content of K 2 O component] 3.0% to 17.0%
- the crystallized inorganic composition article according to any one of Structures 1 to 3 characterized in that: (Composition 5) % by mass of the raw glass in terms of oxide, Total content of Li 2 O component and P 2 O 5 component [content of Li 2 O component + content of P 2 O 5 component] 8.0% to 18.0%
- the raw glass is Composition 1 characterized by not containing TiO 2 , Bi 2 O 3 , Cr 2 O 3 , CuO, La
- Crystallized inorganic composition article according to any one of -5 (Composition 7) % by mass of the raw glass in terms of oxide, [Content of SiO 2 component/Content of ZrO 2 component] is 15.0 to 40.0, The crystallized inorganic composition article according to any one of structures 1 to 6, characterized in that: (Composition 8) % by mass of the raw glass in terms of oxide, [SiO 2 component content/(Na 2 O component content + K 2 O component content)] is 23.0 to less than 100.0; The crystallized inorganic composition article according to any one of structures 1 to 7, characterized in that
- an inorganic material with high mechanical strength that can be used as a cover glass of a smartphone or a glass member of a housing, and excellent transparency even after heat processing.
- a composition article can be provided.
- the crystallized inorganic composition article of the present invention has high strength and is transparent even when heated. Therefore, members of mobile electronic devices such as cover glasses and housings of smartphones, tablet PCs and wearable terminals It can also be used as a member such as a protective protector used in transport aircraft such as cars and airplanes, and a head-up display substrate.
- Crystallized inorganic composition article of the present invention has a transmittance of 50% or more at 550 nm when heated to [At+50]° C., where At (° C.) is the sag point. Also, the raw glass has a specific range of composition. Crystallized inorganic composition articles of the present invention are, for example, crystallized glass. The crystallized glass may be strengthened crystallized glass having a compressive stress layer formed on its surface by various strengthening methods. Various strengthening methods will be described later. The crystallized inorganic composition article of the present invention can be produced by following the production method and examples described below and adjusting the raw material composition and production conditions.
- an amorphous sheet glass is prepared. It is preferable that the sheet glass be shaped so as to have a desired shape or a shape close to the desired shape after being deformed.
- the surface of the sheet glass may be polished to a mirror surface, or may be a surface after grinding.
- the material of the sheet glass may be any glass from which crystals are precipitated by heating, that is, the original glass of the crystallized glass.
- the composition of the raw glass is expressed in mass % in terms of oxide,
- the content of SiO 2 component is 65.0% to 85.0%, Al 2 O 3 component content is 3.0% to 15.0%,
- the content of P 2 O 5 components is more than 0% to 5.0% Li 2 O component content is more than 5.0% to 15.0%,
- the content of ZrO 2 component is 0% to 10.0%
- the content of MgO component is 0% to 5.0%, [Al 2 O 3 component content/(K 2 O component content + MgO component content)] is greater than 0 to 20.0, [Li 2 O component content/MgO component content] is 8.0 or more.
- the raw glass can be easily deformed into a curved shape by thermal processing, and the crystallized glass member can have a high light transmittance in the visible range.
- the content of each component is indicated by mass% in terms of oxide.
- oxide conversion refers to the amount of The amount of oxide of each component contained is expressed in % by mass.
- A% to B% represent from A% to B%.
- the SiO2 component is a skeleton component that constitutes an inorganic composition article, and is an essential component necessary for enhancing stability and precipitating a desired crystal phase.
- the content of the SiO2 component is 85.0% or less, excessive increase in viscosity and deterioration of meltability can be suppressed, and when it is 65.0% or more, the stability of the inorganic composition article can be improved. can improve sexuality. Therefore, the upper limit is preferably 85.0% or less, more preferably 83.0% or less, still more preferably 80.0% or less.
- the lower limit is preferably 65.0% or more, more preferably 68.0% or more, and still more preferably over 70.0%.
- the Al 2 O 3 component is a skeleton component that constitutes the inorganic composition article, and is an essential component necessary for enhancing stability.
- the content of the Al 2 O 3 component is 15.0% or less, deterioration of devitrification resistance (resistance to deterioration of transparency due to crystallization) can be suppressed, and the content is 3.0% or more. If it is, deterioration of stability can be suppressed. Therefore, the upper limit is preferably 15.0% or less, more preferably 13.0% or less, still more preferably less than 12.0%.
- the lower limit is preferably 3.0% or more, more preferably 4.0% or more, more preferably 5.0% or more, more preferably 7.0% or more, more preferably 8.0% or more.
- the P 2 O 5 component is an essential component that promotes crystal formation of the inorganic composition article.
- the content of the P 2 O 5 component is 5.0% or less, phase separation of the glass can be suppressed.
- the upper limit is preferably 5.0% or less, more preferably 4.5% or less, still more preferably 4.0% or less.
- the lower limit can be set to preferably more than 0%, more preferably 0.5% or more, and still more preferably 1.0% or more.
- the Li 2 O component is an essential component that improves the meltability of the base glass and enhances the manufacturability. If the content of the Li 2 O component is 15.0% or less, deterioration of devitrification resistance can be suppressed, and if it exceeds 5.0%, deterioration of viscosity and deterioration of meltability can be suppressed. , can increase manufacturability. Also, a desired crystal phase can be obtained. Therefore, the lower limit is preferably over 5.0%, more preferably 6.0% or more, and even more preferably 7.0% or more. Also, the upper limit is preferably 15.0% or less, more preferably 13.0% or less, still more preferably 12.0% or less.
- the ZrO 2 component can produce the glass according to the present invention even at 0%, but it is a component that acts as a nucleating agent for crystals when the content exceeds 0%.
- the upper limit is preferably 10.0% or less, more preferably 8.0% or less, more preferably 5.0% or less, and even more preferably less than 2.5%.
- the lower limit is preferably 0% or more, more preferably 0.5% or more, more preferably 0.8% or more, more preferably 1.0% or more, and still more preferably more than 1.5%.
- the MgO component can produce the glass according to the present invention even at 0%, but it is a component that improves the low-temperature meltability when it is contained in excess of 0%. If the content of the MgO component is 5.0% or less, it becomes easier to strengthen when performing chemical strengthening. Therefore, the upper limit is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably less than 2.0%. Also, the lower limit is preferably 0% or more, more preferably 0.1% or more, and still more preferably 0.2% or more.
- the ZnO component can produce the glass according to the present invention even at 0%, but is a component that improves the low-temperature meltability when it is contained in an amount exceeding 0%. If the content of the ZnO component is 5.0% or less, it becomes easier to strengthen when performing chemical strengthening. Therefore, the upper limit is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably less than 2.0%. Also, the lower limit is preferably 0% or more, more preferably over 0%, more preferably 0.1% or more, and even more preferably 0.2% or more.
- the CaO component can produce the glass according to the present invention even at 0%. If the content of the CaO component is 5.0% or less, it becomes easier to strengthen when performing chemical strengthening. Therefore, the upper limit is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably less than 1.0%.
- the SrO component and the BaO component can produce the glass according to the present invention even when they are 0%, but when they are contained in excess of 0%, they are components that improve the low-temperature meltability.
- the contents of the SrO component and the BaO component are each 5.0% or less, the steel is easily strengthened during chemical strengthening. Therefore, the upper limit of each of the SrO component and the BaO component is preferably 5.0% or less, more preferably 3.0% or less, and still more preferably 1.0% or less.
- the lower limit of each can be preferably 0% or more, more preferably 0.3% or more, and still more preferably 0.3% or more.
- the upper limit of [CaO component content + MgO component content] is preferably 5.0% or less, more preferably 3.0% or less, more preferably less than 3.0%, and still more preferably 1.0% or less.
- the lower limit of [CaO component content+MgO component content] is preferably 0% or more, more preferably over 0%, more preferably 0.1% or more, and still more preferably 0.2% or more.
- the K 2 O component and the Na 2 O component are components that improve the meltability of the base glass and enhance the manufacturability, respectively.
- contents of the K 2 O component and the Na 2 O component are respectively 5.0% or less, deterioration of devitrification resistance can be suppressed.
- the glass according to the present invention can be produced even when the K 2 O component and the Na 2 O component are each 0%, but when the content exceeds 0%, deterioration of viscosity and deterioration of meltability are suppressed, Manufacturability can be improved. Therefore, the lower limits of the K 2 O component and the Na 2 O component are preferably 0% or more, more preferably 0% or more, more preferably 0.2% or more, and still more preferably 0.3% or more. Further, the K 2 O component and the Na 2 O component preferably have an upper limit of 5.0% or less, more preferably 4.0% or less, more preferably less than 3.0%, and still more preferably 2.0%. Less than
- the Sb 2 O 3 component is a component that functions as a refining agent when producing raw glass. If the Sb 2 O 3 component is excessively contained, the transmittance in the short wavelength region of the visible light region may deteriorate. Therefore, the upper limit is preferably 3.0% or less, more preferably 1.0% or less, more preferably 0.6% or less, and even more preferably 0.5% or less. Also, the lower limit is preferably 0% or more, more preferably 0.03% or more, and still more preferably 0.06% or more.
- the B 2 O 3 component has the effect of lowering the viscosity of the raw glass.
- the content of the B 2 O 3 component is 10.0% or less, deterioration of devitrification resistance can be suppressed.
- the glass according to the present invention can be produced even when the content of the B 2 O 3 component is 0%, but when the content exceeds 0%, deterioration of the viscosity and meltability of the original glass can be suppressed. . Therefore, preferably the upper limit is 10.0% or less, more preferably 8.0% or less, more preferably 7.0% or less, more preferably 5.0% or less, more preferably 4.0% or less, and further Preferably, it can be 3.0% or less.
- the lower limit is preferably 0% or more, more preferably over 0%, more preferably 0.001% or more, more preferably 0.01% or more, more preferably 0.05% or more, more preferably 0.10% % or more, more preferably 0.30% or more.
- the total content of the K 2 O component and the Na 2 O component [the content of the K 2 O component + the content of the Na 2 O component] is 0%, but the glass according to the present invention can be produced. In this case, deterioration of viscosity can be suppressed, and an increase in melting temperature can be suppressed. Moreover, deterioration of devitrification resistance can be suppressed by adjusting the content to 5.0% or less. Therefore, the lower limit of [content of K 2 O component + content of Na 2 O component] is preferably 0% or more, more preferably 0.2% or more, and still more preferably 0.3% or more. Also, the upper limit is preferably 5.0% or less, more preferably 4.0% or less, more preferably less than 4.0%, more preferably less than 3.0%, and even more preferably less than 2.0%.
- the total content of the MgO component, CaO component, SrO component, BaO component and ZnO component is 15.0% or less to facilitate chemical strengthening.
- the glass according to the present invention can be produced even if [MgO component + CaO component + SrO component + BaO component + ZnO component] is 0%, but when it is more than 0%, deterioration of low meltability can be suppressed.
- the lower limit of [MgO component + CaO component + SrO component + BaO component + ZnO component] is preferably 0% or more, more preferably 0% or more, more preferably 0.5% or more, and still more preferably 1.0% or more.
- the upper limit is preferably 15.0% or less, more preferably 10.0% or less, more preferably 5.0% or less, and even more preferably 3.5% or less.
- the preferable upper limit of [content of Al 2 O 3 component/content of K 2 O component] is 100.0 or less, more preferably 80.0 or less, more preferably 60.0 or less, more preferably 40.0 or less. , more preferably 20.0 or less, and still more preferably 15.0 or less.
- the preferable lower limit of [content of Al 2 O 3 component/content of K 2 O component] is 0.6 or more, more preferably 1.0 or more, more preferably 2.0 or more, more preferably 3.0 or more. , more preferably 5.7 or more. Also, the content of the K 2 O component can be zero.
- the upper limit is preferably 20.0 or less, more preferably 18.0 or less, more preferably 16.0 or less, still more preferably 15.0 or less.
- the preferable lower limit of [content of Al 2 O 3 component/(content of K 2 O component + content of MgO component)] is more than 0, more preferably 1.0 or more, more preferably 2.0 or more, and still more preferably 2.6 or higher.
- [Content of Al 2 O 3 components/(Content of ZnO component + Content of MgO component)] is 20.0 or less to suppress deterioration of meltability, and 3.0 or more to prevent loss resistance. Deterioration of permeability can be suppressed. Therefore, the upper limit of [Al 2 O 3 component content/(ZnO component content+MgO component content)] is preferably 20.0 or less, more preferably 18.0 or less, and still more preferably 16.0 or less. Also, the lower limit is preferably 3.0 or more, more preferably 4.0 or more, and still more preferably more than 5.0.
- the preferable upper limit of [Li 2 O component content/MgO component content] is 150.0 or less, more preferably 100.0 or less, more preferably 50.0 or less, more preferably 30.0 or less, and more preferably can be 25.0 or less, more preferably 23.0 or less. Also, MgO can be zero.
- the lower limit of [Li 2 O component content/MgO component content] is preferably 8.0 or more, more preferably 9.0 or more, more preferably 9.5 or more, more preferably 10.0 or more, and further preferably Preferably, it can be 10.6 or more.
- the preferred upper limit of [Li 2 O component content/(MgO component content + CaO component content + SrO component content + BaO component content + Na 2 O component content + K 2 O component content)] is 50.0 or less, More preferably 35.0 or less, more preferably 30.0 or less, more preferably 20.0 or less, more preferably 15.0 or less, more preferably 13.0 or less, still more preferably 10.0 or less can be done.
- [content of Li 2 O component/(content of MgO component + content of CaO component + content of SrO component + content of BaO component + content of Na 2 O component + content of K 2 O component)] can be set to zero.
- the preferred lower limit of [Li 2 O component content/(MgO component content + CaO component content + SrO component content + BaO component content + Na 2 O component content + K 2 O component content)] is 1.0 or more. , more preferably 2.0 or more, more preferably 3.0 or more, and still more preferably more than 3.0.
- [MgO component content/(Li 2 O component content + MgO component content)] is set to 0.6 or less to suppress difficulty in chemical strengthening and to suppress deterioration of devitrification resistance. Even if the lower limit is 0, the glass according to the present invention can be produced. Therefore, the upper limit of [MgO component content/(Li 2 O component content + MgO component content)] is preferably 0.6 or less, more preferably 0.3 or less, and still more preferably less than 0.15. On the other hand, the lower limit of [content of MgO component/(content of Li 2 O component + content of MgO component)] is preferably 0 or more, more preferably 0.01 or more, more preferably 0.03 or more, further preferably 0.03 or more. 04 or more.
- the total content of the Li 2 O component, the Na 2 O component, and the K 2 O component enhances the meltability and facilitates the production of raw glass. It is an indicator of That is, by making it 17.0% or less, deterioration of devitrification resistance can be suppressed, and by making it 3.0% or more, deterioration of viscosity and increase in melting temperature can be suppressed. . Therefore, the upper limit of [Li 2 O component content + Na 2 O component content + K 2 O component content] is preferably 17.0% or less, more preferably 15.0% or less, and still more preferably 14.0% or less. do. Further, the preferable lower limit of [content of Li 2 O component + content of Na 2 O component + content of K 2 O component] is 3.0% or more, more preferably 5.0% or more, further preferably 8.0% or more. can.
- the upper limit of [Li 2 O component content + P 2 O 5 component content] is preferably 18.0% or less, more preferably 17.0% or less, more preferably 15.0% or less, and still more preferably 13.0%. 8% or less.
- the lower limit of [content of Li 2 O component + content of P 2 O 5 component] is preferably 8.0% or more, more preferably 9.0% or more, more preferably 10.0% or more, more preferably 11.0% or more. It can be 5% or more, more preferably 12.01% or more.
- the upper limit of [P 2 O 5 component content/MgO component content] is preferably 50.0 or less, more preferably 30.0 or less, more preferably 10.0 or less, more preferably 5.0 or less, and more preferably 5.0 or less. It is preferably 4.1 or less, more preferably 4.0 or less, still more preferably 3.7 or less. Also, the content of the MgO component can be zero. In addition, the preferable lower limit of [content of P 2 O 5 component/content of MgO component] is more than 0, more preferably 0.02 or more, more preferably 0.1 or more, more preferably 0.15 or more, and still more preferably 2.4 or higher.
- the upper limit of [content of SiO 2 component/content of ZrO 2 component] is preferably 40.0 or less, more preferably 37.0 or less, more preferably 35.4 or less, more preferably 35.0 or less, and more preferably is 33.7 or less, more preferably 32.7 or less.
- the preferable lower limit of [content of SiO 2 component/content of ZrO 2 component] is 15.0 or more, more preferably 17.0 or more, more preferably 18.0 or more, more preferably 19.6 or more, and even more preferably can be 29.9 or more.
- the upper limit of [SiO 2 component content/Li 2 O component content] is preferably 17.0 or less, more preferably 15.0 or less, more preferably 13.0 or less, more preferably 10.0 or less, and more preferably 10.0 or less. It is preferably 9.0 or less, more preferably 7.6 or less.
- the lower limit of [content of SiO 2 component/content of Li 2 O component] is preferably 4.0 or more, more preferably 4.3 or more, and still more preferably 5.0 or more.
- the upper limit of [content of SiO 2 component/content of P 2 O 5 component] is preferably 100.0 or less, more preferably 80.0 or less, more preferably 50.0 or less, more preferably 40.0 or less. It is more preferably 39.0 or less.
- the preferable lower limit of [content of SiO 2 component/content of P 2 O 5 component] is 13.0 or more, more preferably 17.0 or more, more preferably 20.0 or more, more preferably 30.0 or more, More preferably, it can be 33.0 or more.
- [Content of SiO 2 component/(Content of P 2 O 5 component + Content of ZrO 2 component)] is 100.0 or less to obtain the desired crystal phase, and 4.3 or more Deterioration of devitrification resistance can be suppressed. Therefore, the upper limit of [content of SiO 2 component/(content of P 2 O 5 component + content of ZrO 2 component)] is preferably 100.0 or less, more preferably 80.0 or less, more preferably 50.0 or less, and more preferably It is preferably 42.5 or less, more preferably 35.0 or less, more preferably 20.0 or less, still more preferably 17.99 or less.
- the preferable lower limit of [content of SiO 2 component/(content of P 2 O 5 component + content of ZrO 2 component)] is 4.3 or more, more preferably 10.0 or more, more preferably 15.0 or more. Preferably, it can be 16.1 or more.
- [Content of SiO 2 component/(Content of Na 2 O component + Content of K 2 O component)] is set to be less than 100.0 to suppress deterioration of low-temperature meltability, and is set to 23.0 or more. A desired crystal phase can be obtained by this. Therefore, the upper limit of [SiO 2 component content/(Na 2 O component content + K 2 O component content)] is preferably less than 100.0%, more preferably 90.0% or less, and still more preferably 80.0% or less. and in addition, the preferable lower limit of [content of SiO 2 component/(content of Na 2 O component + content of K 2 O component)] is 23.0 or more, more preferably 25.0 or more, more preferably 30.0 or more, and more preferably 30.0 or more. It is preferably 35.0 or more, more preferably 54.0 or more.
- [ZnO component content/(Li 2 O component content + P 2 O 5 component content + MgO component content)] is 1.0 or less to obtain a desired crystal phase, and the lower limit is 0.
- the upper limit of [ZnO component content/(Li 2 O component content + P 2 O 5 component content + MgO component content)] is preferably 1.0 or less, more preferably 0.09 or less, and more preferably 0.09 or less. 06 or less, more preferably 0.05 or less.
- the preferable lower limit of [ZnO component content/(Li 2 O component content + P 2 O 5 component content + MgO component content)] is 0 or more, more preferably 0 or more, more preferably 0.01 or more, and more It is preferably 0.02 or more, more preferably 0.03 or more.
- [(content of SiO 2 component + content of Al 2 O 3 component + content of P 2 O 5 component)/(content of Li 2 O component + content of Na 2 O component + content of K 2 O component + content of MgO component)] is When it is 9.0 or less, deterioration of low-temperature meltability can be suppressed, and when it is 0.7 or more, crystal precipitation can be promoted. Therefore, [(content of SiO 2 component + content of Al 2 O 3 component + content of P 2 O 5 component)/(content of Li 2 O component + content of Na 2 O component + content of K 2 O component + content of MgO component)] is preferably 9.0 or less, more preferably 8.0 or less, still more preferably less than 7.25.
- [(content of SiO 2 component + content of Al 2 O 3 component + content of P 2 O 5 component)/(content of Li 2 O component + content of Na 2 O component + content of K 2 O component + content of MgO component)]. is preferably 0.7 or more, more preferably 4.0 or more, more preferably 5.0 or more, and still more preferably 6.0 or more.
- the inorganic composition article (for example, crystallized glass) of the present invention contains TiO 2 , Bi 2 O 3 , Cr 2 O 3 , CuO, La 2 O 3 , MnO, MoO 3 , PbO, V 2 O 5 , WO 3 and Y 2 O 3 components may or may not be included. Not containing these components has the effect of preventing the transmittance from deteriorating.
- the crystallized glass may or may not contain other components not mentioned above as long as the characteristics of the crystallized glass of the present invention are not impaired.
- examples include metal components such as Yb, Lu, Fe, Co, Ni and Ag (including metal oxides thereof).
- the glass clarifier may contain one or more selected from the group consisting of two SnO components, two CeO components, three As 2 O components, and F, NOx, and SOx. and may not be included.
- the upper limit of the content of the fining agent is preferably 3.0% or less, more preferably 2.0% or less, more preferably 1.0% or less, and most preferably 0.6% or less.
- Crystallized glass can be produced by the following method. That is, raw materials are uniformly mixed so that the content of each component falls within a predetermined range, and the mixture is melt-molded to produce raw glass. Next, this raw glass is crystallized to produce crystallized glass.
- the heat treatment for crystal precipitation may be performed in one stage or in two stages of temperature.
- the nucleation step is first performed by heat treatment at a first temperature, and after this nucleation step, the crystal growth step is performed by heat treatment at a second temperature higher than the nucleation step.
- the first temperature of the two-stage heat treatment is preferably 400°C to 750°C, more preferably 450°C to 720°C, and even more preferably 500°C to 680°C.
- the holding time at the first temperature is preferably 30 minutes to 2000 minutes, more preferably 180 minutes to 1440 minutes.
- the second temperature of the two-step heat treatment is preferably 550°C to 850°C, more preferably 600°C to 800°C.
- the retention time at the second temperature is preferably 30 minutes to 600 minutes, more preferably 60 minutes to 400 minutes.
- the nucleation step and the crystal growth step are performed continuously at one step of temperature.
- the temperature is raised to a predetermined heat treatment temperature, and after reaching the heat treatment temperature, the temperature is maintained for a certain period of time, and then the temperature is lowered.
- the heat treatment temperature is preferably 600°C to 800°C, more preferably 630°C to 770°C.
- the holding time at the heat treatment temperature is preferably 30 minutes to 500 minutes, more preferably 60 minutes to 400 minutes.
- the inorganic composition articles of the present invention comprise one or more crystalline phases selected from lithium disilicate, petalite, vergilite, beta-quartz and lithium monosilicate. By having these crystalline phases, it is possible to obtain an inorganic composition article having high strength and high transmittance even when heat processing is performed.
- the inorganic composition articles of the present invention comprise crystalline phases of lithium disilicate, petalite, vergilite, and lithium monosilicate.
- the inorganic composition article of the present invention comprises crystalline phases of lithium disilicate, petalite, and vergilite.
- the inorganic composition articles of the present invention comprise crystalline phases of lithium disilicate, petalite, and lithium monosilicate. In one aspect, the inorganic composition article of the present invention comprises a crystalline phase of petalite. The method for confirming the crystal phase is as described in Examples.
- the inorganic composition article of the present invention has a transmittance at 550 nm (after) of 50% or more when heated to [At+50]° C., where At (° C.) is the sag point.
- the yield point and transmittance are measured by the methods described in Examples.
- the transmittance at 550 nm of the inorganic composition article of the present invention after heating to [At+50]° C. may be 55% or more, 60% or more, 65% or more, or 70% or more.
- the transmittance at 550 nm of the inorganic composition article of the present invention after heating to At° C. is, for example, 80% or more, 85% or more, or 90% or more.
- the difference between the transmittance at 550 nm after heating to [At + 50] ° C. and the transmittance at 550 nm when heated to At ° C. of the inorganic composition article of the present invention is, for example, 36% or less, 35% or less, It is 30% or less, or 25% or less, and can maintain a high transmittance even after thermal processing.
- the inorganic composition article of the present invention may or may not be subjected to strengthening treatment such as chemical strengthening.
- a strengthening treatment usually forms a compressive stress layer on the surface of the crystallized glass. Crystallized glass that has been tempered is also referred to as “strengthened crystallized glass”.
- a method for forming a compressive stress layer in strengthened crystallized glass for example, an alkali component present in the surface layer of the crystallized glass is exchange-reacted with an alkali component having a larger ionic radius to form a compressive stress layer on the surface layer.
- a chemical strengthening method for example, There are also a thermal strengthening method in which crystallized glass is heated and then rapidly cooled, and an ion implantation method in which ions are implanted into the surface layer of crystallized glass.
- the chemical strengthening method can be carried out, for example, by the following steps. Crystallized glass is brought into contact with or immersed in a molten salt containing potassium or sodium, such as potassium nitrate (KNO 3 ), sodium nitrate (NaNO 3 ), or a mixed salt or composite salt thereof.
- a molten salt containing potassium or sodium such as potassium nitrate (KNO 3 ), sodium nitrate (NaNO 3 ), or a mixed salt or composite salt thereof.
- KNO 3 potassium nitrate
- NaNO 3 sodium nitrate
- the treatment of contacting or immersing in the molten salt may be performed in one step or in two steps.
- the steel is contacted or immersed in a sodium salt or a mixed salt of potassium and sodium heated at 350° C. to 550° C. for 1 to 1440 minutes, preferably 30 to 500 minutes.
- the one-step chemical strengthening treatment it is brought into contact with or immersed in a salt containing potassium or sodium heated at 350° C. to 550° C. or a mixed salt thereof for 1 to 1440 minutes.
- the thermal strengthening method is not particularly limited, but for example, after heating the crystallized glass to 300° C. to 600° C., the temperature difference between the surface and the inside of the glass is reduced by performing rapid cooling such as water cooling and / or air cooling. can form a compressive stress layer. By combining with the above chemical treatment method, the compressive stress layer can be formed more effectively.
- the ion implantation method is not particularly limited, but for example, ions are implanted into the crystallized glass surface by colliding arbitrary ions with an acceleration energy and an acceleration voltage that do not destroy the surface.
- a compressive stress layer can be formed on the surface in the same manner as in other methods by performing heat treatment as necessary thereafter.
- Examples 1 to 4 Comparative Example 1 1.
- Manufacture of crystallized glass As raw materials for each component of crystallized glass, raw materials for corresponding compounds are selected, and these raw materials are weighed and uniformly mixed so that the composition shown in Table 1 is obtained when converted to oxides. Mixed.
- the mixed raw materials were put into a platinum crucible and melted in an electric furnace at 1300°C to 1600°C for 2 to 24 hours depending on the melting difficulty of the glass composition. Thereafter, the molten glass was stirred and homogenized, cooled to 1000° C. to 1450° C., cast into a mold, and gradually cooled to prepare a raw glass.
- the raw glass thus obtained was heated under the nucleation conditions and crystallization conditions shown in Table 2 to produce crystallized glass. In Table 2, a blank indicates that the corresponding step was not performed.
- crystal phase of crystallized glass was measured using an X-ray diffraction analyzer (D8Discover, manufactured by Bruker). It was determined from the intensity ratio of diffraction peaks. At this time, from the X-ray diffraction patterns of the crystallized glasses of Examples 1 to 4 and Comparative Example 1, the crystallized glasses are selected from lithium disilicate, petalite, vergilite, ⁇ -quartz and lithium monosilicate. It was confirmed that more than seeds were included in the crystal phase.
- Example 1 to 4 and Comparative Example 1 A crystallized glass substrate was obtained by cutting and grinding the crystallized glass produced in 1. and polishing the crystallized glass so as to have a thickness of 1.0 mm.
- this crystallized glass substrate was used as a base material and chemically strengthened to obtain inorganic composition articles.
- Table 2 shows the production conditions (strengthening conditions) of the inorganic composition article.
- the description of “Na alone A° C. Bhr” in the tempering conditions means that the crystallized glass substrate is immersed in a molten salt of sodium nitrate (NaNO 3 ) heated at a temperature of A° C. for B hours.
- the crystallized glass substrate was used as an inorganic composition article.
- the value of the refractive index at a wavelength of 405 nm is a second-order approximation from the measured values of the refractive index at the wavelengths of the C-line, d-line, F-line, and g-line according to the V-block method specified in JIS B 7071-2: 2018. Calculated using the formula.
- the photoelastic constant ( ⁇ ) at a wavelength of 405 nm used for CS, DOLzero and CT measurements is calculated using a quadratic approximation from the measured values of the photoelastic constant at a wavelength of 435.8 nm, a wavelength of 546.1 nm, and a wavelength of 643.9 nm. can. 27.3 was used as a representative value in the examples.
- the photoelastic constant ( ⁇ ) was obtained by polishing the sample shape to a disk shape with a diameter of 25 mm and a thickness of 8 mm, applying a compressive load in a predetermined direction, and measuring the optical path difference occurring at the center of the glass. It was obtained from the relational expression of d ⁇ F. In this relational expression, the optical path difference is expressed as ⁇ (nm), the glass thickness as d (cm), and the stress as F (MPa).
- Example 2 will be specifically described.
- the crystallized glass thin plate produced in Example 2 was held in a furnace (SK-3035F furnace manufactured by Motoyama) in which the temperature was set at 771° C. (that is, At in Example 2) for 0.5 hours, and then It was taken out from the container and allowed to cool naturally.
- Example 2 the crystallized glass thin plate produced in Example 2 was held in a furnace (SK-3035F furnace manufactured by Motoyama Co., Ltd.) at 821°C (that is, At + 50°C in Example 2) for 0.5 hours, and then removed from the furnace. It was allowed to cool naturally.
- SK-3035F furnace manufactured by Motoyama Co., Ltd.
- the same thin plate heat treatment as in Example 2 was performed.
- the inorganic composition articles of Examples 1 to 4 and Comparative Example 1 were evaluated as follows. Table 2 shows the results. In Table 2, a blank indicates that the corresponding measurement was not performed.
- the object was the inorganic composition article obtained in .
- the Vickers hardness is the surface area (mm 2 ) calculated from the length of a pyramid-shaped indentation on the test surface using a diamond square pyramid indenter with a facing angle of 136 °. It is shown as a divided value. Measurement was performed using a Micro Vickers Hardness Tester HMV-G21D manufactured by Shimadzu Corporation under a test load of 100 gf and a holding time of 10 seconds.
- the inorganic composition article obtained in 1. it was measured by an ultrasonic method.
- the object was the inorganic composition article obtained in .
- the light transmittance including reflection loss at a thickness of 1 mm was measured with a spectrophotometer (U-4000, manufactured by Hitachi High Technology).
- a wavelength ⁇ 5 (nm) at which the transmittance is 5% and a wavelength ⁇ 80 (nm) at which the transmittance is 80% were obtained.
- the light transmittance (%) was measured for the two crystallized glass thin plates subjected to the thin plate heat treatment, that is, the one heat-treated at At (° C.) and the one heat-treated at At+50 (° C.). Specifically, the light transmittance (%) including the reflection loss at 550 nm was measured at room temperature with a spectrophotometer (U-4000, manufactured by Hitachi High Technology). The light transmittance (%) of the crystallized glass thin plate subjected to thin plate heat treatment is the same regardless of the presence or absence of chemical strengthening treatment in thin plate heat treatment.
- Table 2 shows the above results. From the results in Table 2, it can be seen that the inorganic composition article of the present invention is a material having high transmittance even after thermal processing.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Ceramic Engineering (AREA)
- Life Sciences & Earth Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- General Chemical & Material Sciences (AREA)
- Geochemistry & Mineralogy (AREA)
- Materials Engineering (AREA)
- Organic Chemistry (AREA)
- Crystallography & Structural Chemistry (AREA)
- Dispersion Chemistry (AREA)
- Glass Compositions (AREA)
Priority Applications (5)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| EP23747175.0A EP4474361A4 (en) | 2022-01-31 | 2023-01-31 | CRYSTALLIZED INORGANIC COMPOSITION ARTICLE |
| JP2023528638A JPWO2023145965A1 (cg-RX-API-DMAC7.html) | 2022-01-31 | 2023-01-31 | |
| CN202380018486.9A CN118591515A (zh) | 2022-01-31 | 2023-01-31 | 经结晶化的无机组成物产品 |
| KR1020247025931A KR20240144183A (ko) | 2022-01-31 | 2023-01-31 | 결정화된 무기 조성물 물품 |
| US18/834,614 US20250122116A1 (en) | 2022-01-31 | 2023-01-31 | Crystallized inorganic composition article |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022-012978 | 2022-01-31 | ||
| JP2022012978 | 2022-01-31 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023145965A1 true WO2023145965A1 (ja) | 2023-08-03 |
Family
ID=87471781
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/003045 Ceased WO2023145965A1 (ja) | 2022-01-31 | 2023-01-31 | 結晶化された無機組成物物品 |
Country Status (7)
| Country | Link |
|---|---|
| US (1) | US20250122116A1 (cg-RX-API-DMAC7.html) |
| EP (1) | EP4474361A4 (cg-RX-API-DMAC7.html) |
| JP (1) | JPWO2023145965A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20240144183A (cg-RX-API-DMAC7.html) |
| CN (1) | CN118591515A (cg-RX-API-DMAC7.html) |
| TW (1) | TW202337860A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023145965A1 (cg-RX-API-DMAC7.html) |
Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2001048584A (ja) | 1999-08-10 | 2001-02-20 | Ohara Inc | 光フィルター用ガラスセラミックス及び光フィルター |
| JP2001097739A (ja) * | 1999-09-29 | 2001-04-10 | Ngk Insulators Ltd | 結晶化ガラスの製造方法 |
| JP2001126236A (ja) * | 1999-10-25 | 2001-05-11 | Ngk Insulators Ltd | 磁気ディスク用基板および磁気ディスク |
| JP2008254984A (ja) | 2007-04-06 | 2008-10-23 | Ohara Inc | 無機組成物物品 |
| WO2019167850A1 (ja) * | 2018-02-27 | 2019-09-06 | Agc株式会社 | 3次元形状の結晶化ガラス、3次元形状の化学強化ガラスおよびそれらの製造方法 |
| JP2020019659A (ja) | 2018-07-30 | 2020-02-06 | 株式会社オハラ | 結晶化ガラス |
| JP2021509658A (ja) * | 2017-12-01 | 2021-04-01 | シーディージーエム グラス カンパニー リミテッド | 結晶化ガラスおよびその基板 |
| JP2021095333A (ja) | 2014-10-08 | 2021-06-24 | コーニング インコーポレイテッド | ペタライト及びリチウムシリケート構造を有する高強度ガラスセラミック |
Family Cites Families (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6677259B2 (en) * | 1999-08-10 | 2004-01-13 | Kabushiki Kaisha Ohara | Glass-ceramics for a light filter |
| US6426311B1 (en) * | 2000-02-01 | 2002-07-30 | Kabushiki Kaisha Ohara | Glass-ceramics |
| JP4704585B2 (ja) * | 2000-07-07 | 2011-06-15 | 株式会社オハラ | 低膨張透明結晶化ガラス、結晶化ガラス基板及び光導波路素子 |
| US20020115550A1 (en) * | 2000-08-11 | 2002-08-22 | Hideki Kawai | Substrate made of glass ceramics |
| PT1688398E (pt) * | 2005-02-08 | 2014-07-25 | Ivoclar Vivadent Ag | Vitrocerâmica de silicato de lítio |
| JP4755135B2 (ja) * | 2007-04-27 | 2011-08-24 | 株式会社オハラ | 結晶化ガラス |
| JP5070006B2 (ja) * | 2007-11-02 | 2012-11-07 | 株式会社オハラ | 結晶化ガラス |
| DE202009019061U1 (de) * | 2009-12-23 | 2016-02-23 | Degudent Gmbh | Lithiummetasilicat-Glaskeramik und deren Verwendung |
| JP2015110508A (ja) * | 2013-10-31 | 2015-06-18 | 株式会社オハラ | 結晶化ガラス |
| JP6953101B2 (ja) * | 2017-02-24 | 2021-10-27 | 株式会社オハラ | 結晶化ガラス |
| JP7004234B2 (ja) * | 2017-05-30 | 2022-01-21 | 日本電気硝子株式会社 | 支持結晶化ガラス基板の製造方法 |
| CN111268913B (zh) * | 2018-10-26 | 2022-07-29 | 成都光明光电股份有限公司 | 电子设备盖板用微晶玻璃制品和微晶玻璃 |
| JP6903815B2 (ja) * | 2019-03-29 | 2021-07-14 | 株式会社ジーシー | 歯科補綴物用ブロック体 |
| CN113248152B (zh) * | 2021-05-21 | 2022-06-10 | 常熟佳合显示科技有限公司 | 一种三维微晶玻璃及其制备方法 |
-
2023
- 2023-01-31 KR KR1020247025931A patent/KR20240144183A/ko active Pending
- 2023-01-31 TW TW112103371A patent/TW202337860A/zh unknown
- 2023-01-31 JP JP2023528638A patent/JPWO2023145965A1/ja active Pending
- 2023-01-31 EP EP23747175.0A patent/EP4474361A4/en active Pending
- 2023-01-31 WO PCT/JP2023/003045 patent/WO2023145965A1/ja not_active Ceased
- 2023-01-31 US US18/834,614 patent/US20250122116A1/en active Pending
- 2023-01-31 CN CN202380018486.9A patent/CN118591515A/zh active Pending
Patent Citations (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2001048584A (ja) | 1999-08-10 | 2001-02-20 | Ohara Inc | 光フィルター用ガラスセラミックス及び光フィルター |
| JP2001097739A (ja) * | 1999-09-29 | 2001-04-10 | Ngk Insulators Ltd | 結晶化ガラスの製造方法 |
| JP2001126236A (ja) * | 1999-10-25 | 2001-05-11 | Ngk Insulators Ltd | 磁気ディスク用基板および磁気ディスク |
| JP2008254984A (ja) | 2007-04-06 | 2008-10-23 | Ohara Inc | 無機組成物物品 |
| JP2021095333A (ja) | 2014-10-08 | 2021-06-24 | コーニング インコーポレイテッド | ペタライト及びリチウムシリケート構造を有する高強度ガラスセラミック |
| JP2021100909A (ja) * | 2014-10-08 | 2021-07-08 | コーニング インコーポレイテッド | ペタライト及びリチウムシリケート構造を有する高強度ガラスセラミック |
| JP2021509658A (ja) * | 2017-12-01 | 2021-04-01 | シーディージーエム グラス カンパニー リミテッド | 結晶化ガラスおよびその基板 |
| WO2019167850A1 (ja) * | 2018-02-27 | 2019-09-06 | Agc株式会社 | 3次元形状の結晶化ガラス、3次元形状の化学強化ガラスおよびそれらの製造方法 |
| JP2020019659A (ja) | 2018-07-30 | 2020-02-06 | 株式会社オハラ | 結晶化ガラス |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP4474361A4 |
Also Published As
| Publication number | Publication date |
|---|---|
| EP4474361A4 (en) | 2026-01-28 |
| US20250122116A1 (en) | 2025-04-17 |
| KR20240144183A (ko) | 2024-10-02 |
| TW202337860A (zh) | 2023-10-01 |
| CN118591515A (zh) | 2024-09-03 |
| EP4474361A1 (en) | 2024-12-11 |
| JPWO2023145965A1 (cg-RX-API-DMAC7.html) | 2023-08-03 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7600089B2 (ja) | 無機組成物物品および結晶化ガラス | |
| JP7770892B2 (ja) | 結晶化ガラスおよび強化結晶化ガラス | |
| JP7703711B2 (ja) | 結晶化ガラスおよび強化結晶化ガラス | |
| JP7802535B2 (ja) | 無機組成物物品 | |
| JP7721440B2 (ja) | 強化結晶化ガラス | |
| JP7189181B2 (ja) | ガラスおよび結晶化ガラス | |
| JP7732739B2 (ja) | 結晶化ガラスおよび強化結晶化ガラス | |
| TWI912550B (zh) | 結晶化玻璃 | |
| WO2023145956A1 (ja) | 無機組成物物品 | |
| WO2023095454A1 (ja) | 無機組成物物品 | |
| US20250122116A1 (en) | Crystallized inorganic composition article | |
| WO2024190443A1 (ja) | 結晶化ガラス | |
| WO2024062797A1 (ja) | 結晶化ガラス | |
| WO2024225266A1 (ja) | 無機組成物物品 | |
| WO2024143174A1 (ja) | 無機組成物物品 | |
| WO2024014500A1 (ja) | 無機組成物物品 | |
| WO2024014507A1 (ja) | 無機組成物物品 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023528638 Country of ref document: JP |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23747175 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202380018486.9 Country of ref document: CN |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 18834614 Country of ref document: US |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023747175 Country of ref document: EP |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| ENP | Entry into the national phase |
Ref document number: 2023747175 Country of ref document: EP Effective date: 20240902 |
|
| WWP | Wipo information: published in national office |
Ref document number: 18834614 Country of ref document: US |