WO2023090130A1 - 光輝性塗料組成物、及び複層塗膜形成方法 - Google Patents
光輝性塗料組成物、及び複層塗膜形成方法 Download PDFInfo
- Publication number
- WO2023090130A1 WO2023090130A1 PCT/JP2022/040487 JP2022040487W WO2023090130A1 WO 2023090130 A1 WO2023090130 A1 WO 2023090130A1 JP 2022040487 W JP2022040487 W JP 2022040487W WO 2023090130 A1 WO2023090130 A1 WO 2023090130A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- coating composition
- glitter
- coating film
- parts
- glitter coating
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
- C09D5/22—Luminous paints
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/02—Processes for applying liquids or other fluent materials performed by spraying
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/26—Processes for applying liquids or other fluent materials performed by applying the liquid or other fluent material from an outlet device in contact with, or almost in contact with, the surface
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/36—Successively applying liquids or other fluent materials, e.g. without intermediate treatment
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D3/00—Pretreatment of surfaces to which liquids or other fluent materials are to be applied; After-treatment of applied coatings, e.g. intermediate treating of an applied coating preparatory to subsequent applications of liquids or other fluent materials
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D5/00—Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures
- B05D5/06—Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures to obtain multicolour or other optical effects
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D5/00—Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures
- B05D5/06—Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures to obtain multicolour or other optical effects
- B05D5/067—Metallic effect
- B05D5/068—Metallic effect achieved by multilayers
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D7/00—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials
- B05D7/24—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials for applying particular liquids or other fluent materials
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09C—TREATMENT OF INORGANIC MATERIALS, OTHER THAN FIBROUS FILLERS, TO ENHANCE THEIR PIGMENTING OR FILLING PROPERTIES ; PREPARATION OF CARBON BLACK ; PREPARATION OF INORGANIC MATERIALS WHICH ARE NO SINGLE CHEMICAL COMPOUNDS AND WHICH ARE MAINLY USED AS PIGMENTS OR FILLERS
- C09C1/00—Treatment of specific inorganic materials other than fibrous fillers; Preparation of carbon black
- C09C1/62—Metallic pigments or fillers
- C09C1/64—Aluminium
- C09C1/644—Aluminium treated with organic compounds, e.g. polymers
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D101/00—Coating compositions based on cellulose, modified cellulose, or cellulose derivatives
- C09D101/02—Cellulose; Modified cellulose
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D133/00—Coating compositions based on homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Coating compositions based on derivatives of such polymers
- C09D133/04—Homopolymers or copolymers of esters
- C09D133/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, the oxygen atom being present only as part of the carboxyl radical
- C09D133/08—Homopolymers or copolymers of acrylic acid esters
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D201/00—Coating compositions based on unspecified macromolecular compounds
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
- C09D5/02—Emulsion paints including aerosols
- C09D5/024—Emulsion paints including aerosols characterised by the additives
- C09D5/028—Pigments; Filters
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/60—Additives non-macromolecular
- C09D7/61—Additives non-macromolecular inorganic
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/65—Additives macromolecular
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/66—Additives characterised by particle size
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/70—Additives characterised by shape, e.g. fibres, flakes or microspheres
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/51—Particles with a specific particle size distribution
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/60—Particles characterised by their size
- C01P2004/61—Micrometer sized, i.e. from 1-100 micrometer
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/60—Particles characterised by their size
- C01P2004/62—Submicrometer sized, i.e. from 0.1-1 micrometer
Definitions
- the present disclosure relates to a glitter coating composition and a method for forming a multilayer coating film using the glitter coating composition.
- Patent Document 1 describes an image forming step of ejecting effect pigment ink onto a recording medium to form an image, a transparent ink applying step of applying transparent ink onto the recording medium, and It has a curing step of curing the effect pigment ink and the transparent ink in this order, and does not have a step of curing the effect pigment ink between the image forming step and the transparent ink applying step, or if it has a step of curing the effect pigment ink.
- the transparent ink contains a polymerization initiator and a polymerizable compound, and contains substantially no pigment
- the effect pigment ink is An ink jet recording method (claim 1) characterized by containing an effect pigment, a polymerization initiator, and a polymerizable compound is disclosed.
- Patent Document 1 discloses that the effect pigment ink is formed by an inkjet method (paragraph [0020]), and that the effect pigment is preferably aluminum or an aluminum alloy (paragraph [0104]).
- Patent Literature 2 discloses a decorative structure in which the glitter of a glitter material contained in a glitter coating film can be seen through an ink layer, and a manufacturing method thereof.
- the decorative structure according to Patent Document 2 is a decorative structure comprising a substrate, a glitter coating film formed on the substrate, and a transparent ink layer formed on the glitter coating film.
- the glitter coating film contains a glitter material having an average particle diameter of 3 to 100 ⁇ m (claim 1).
- the effect pigment ink is applied by an inkjet method. is likely to occur.
- the glitter coating itself is not coated by an inkjet method, and the glitter is maintained by providing a transparent ink layer on the glitter coating. It is. Therefore, the present disclosure is applicable not only to robot coating, but also to coating using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, so that the formed coating film has a metallic luster. To provide a lustrous coating composition which is excellent in brilliance and is less likely to cause unevenness.
- the present disclosure discloses a glitter coating composition containing water, a scaly aluminum pigment (A) and nanocellulose (B), wherein the scaly aluminum pigment (A) has a thickness of 0.5 to 8.0 ⁇ m and d90 in the range of 2.0 to 15.0 ⁇ m.
- the glitter coating composition of the present disclosure is used not only in robot coating, but also in coating using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port. has excellent metallic luster and is less likely to cause unevenness.
- the scaly aluminum pigment (A) has a volume average particle diameter of d50 in the range of 0.5 to 8.0 ⁇ m and d90 in the range of 2.0 to 15.0 ⁇ m, Glitter paint composition.
- the scale-like aluminum pigment (A) since the scale-like aluminum pigment (A) has a predetermined volume average particle diameter, it can be applied not only by robot coating but also by changing the relative distance between the valve body and the ejection port. In coating using a liquid ejection head that controls ejection, a coating film formed from the glitter coating composition has excellent metallic luster and is less likely to cause unevenness. Further, in the glitter coating composition, since the scale-like aluminum pigment (A) has a predetermined volume average particle diameter, the discharge is controlled by changing the relative distance between the valve body and the discharge port. When applied using a liquid ejection head, the glitter coating composition exhibits excellent ejection stability.
- metallic luster means that the surface does not have a grainy feel like a mirror surface, and when viewed from a nearly vertical position (highlight) to the coated plate, it shines brightly, and when viewed diagonally from above the coated plate.
- shade means a texture that looks dark, that is, is characterized by a large luminance difference between a highlight area and a shaded area.
- the coating film formed from the glitter coating composition has excellent metallic luster.
- the glitter coating composition is applied using a predetermined liquid ejection head, it is excellent in ejection stability when ejected from the liquid ejection head, and is formed from the glitter coating composition.
- the coating film has excellent metallic luster and is less likely to cause unevenness.
- the coating formed from the glitter coating composition since the nanocellulose (B) contains at least one selected from cellulose nanofibers (B1) and cellulose nanocrystals (B2), the coating formed from the glitter coating composition The film has excellent metallic luster. Further, when the glitter coating composition is applied using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, the glitter coating composition The composition has excellent ejection stability.
- the glitter coating composition Since the glitter coating composition has a predetermined solid content concentration, it is excellent in coating stability when applied (particularly, ejection stability when ejected from the liquid ejection head), and the glitter coating A coating film formed from the composition is excellent in metallic luster.
- Step 1 Using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, apply the glitter coating composition according to any one of aspects 1 to 6.
- Step 2 A step of applying a clear coating composition to the glitter coating film to form a clear coating film
- a method for forming a multilayer coating film comprising:
- the method for forming a multi-layer coating film is excellent in ejection stability of the glitter coating composition, and the coating film formed from the glitter coating composition is excellent in metallic luster.
- the glitter coating composition of the present disclosure contains water, scale-like aluminum pigment (A) and nanocellulose (B).
- the scale-like aluminum pigment (A) has a d50 (volume average particle diameter) in the range of 0.5 to 8.0 ⁇ m, preferably 0.5 to 6.0 ⁇ m, and more preferably 0.5 to 4.0 ⁇ m. have.
- the scaly aluminum pigment (A) has a particle diameter of 2.0 to 15.0 ⁇ m, preferably 2.0 to 10.0 ⁇ m, and more preferably 2.0 to 15.0 ⁇ m, provided that it is larger than d50 (volume average particle diameter). It has a d90 (volume average particle size) in the range of 0-7.0 ⁇ m.
- the coating film formed from the glitter coating composition has excellent metallic luster and is less likely to cause unevenness. Further, when the glitter coating composition is applied using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, the glitter coating composition The composition has excellent ejection stability.
- d50 volume average particle diameter
- d90 volume average particle diameter
- scaly aluminum pigment (A) examples include a milling type scaly aluminum pigment and a vapor deposition type scaly aluminum pigment.
- Milling-type scaly aluminum pigments are generally produced by pulverizing and grinding aluminum in a ball mill or attritor mill in the presence of a grinding medium using a grinding aid. Grinding aids used in the manufacturing process of milling-type flaky aluminum pigments include higher fatty acids such as oleic acid, stearic acid, isostearic acid, lauric acid, palmitic acid, and myristic acid, as well as aliphatic amines, aliphatic amides, and fatty acids. family alcohols. Grinding media include aliphatic hydrocarbons such as mineral spirits.
- the scale-like aluminum pigment (A) can be broadly classified into a leafing type and a non-leafing type depending on the type of grinding aid.
- the leafing type when contained in the luster coating composition, arranges (leafing) on the surface of the coating film obtained by coating, gives a finish with a strong metallic feeling, has a heat reflection effect, and has an antirust effect. It is often used for tanks, ducts, pipes, factory equipment such as rooftop roofing, and various building materials.
- Leafing type scaly aluminum pigments can be used as the scaly aluminum pigments used in the glitter coating composition of the present disclosure.
- the surface tension of the pulverization aid causes the particles to be oriented on the surface of the coating film. From this point, it is preferable to use a non-leafing type scale-like aluminum pigment.
- Non-leafing type scaly aluminum pigments include those whose surfaces are not treated, those whose surfaces are coated with resin, those whose surfaces are treated with silica, and those whose surfaces are treated with phosphoric acid, molybdic acid, silane coupling agents, etc. can be used.
- the surface of the scaly aluminum pigment is coated with a coloring pigment and then coated with a resin, and the surface of the scaly aluminum pigment is coated with a metal oxide such as iron oxide.
- Colored aluminum pigments such as those can be employed.
- the scaly aluminum pigment (A) preferably has an average thickness of 1-100 nm, more preferably 2-60 nm, and even more preferably 3-50 nm.
- the average thickness is defined as the average value of 100 or more measured values obtained by observing the cross section of the coating film containing the scale-like aluminum pigment (A) with a microscope and measuring the thickness using image processing software.
- a vapor deposition type scale-like aluminum pigment can be obtained by vapor-depositing an aluminum film on a base material, peeling off the base material, and pulverizing the vapor-deposited aluminum film.
- the base material include films.
- the vapor deposition type scale-like aluminum pigment includes not only a single layer type having a single layer vapor deposition aluminum film, but also a multilayer type having a further layer of other metals, metal oxides, etc. on the single layer vapor deposition aluminum film. type can be used.
- Various surface-treated aluminum pigments can also be used for vapor deposition type scale-like aluminum pigments, but from the viewpoint of the storage stability of the luster pigment dispersion, it is particularly preferable to use those treated with silica. is.
- the glitter coating composition of the present disclosure contains the scale-like aluminum pigment (A), based on the total mass of the glitter coating composition, preferably from 0.3 to 10.0 mass %, more preferably 0.7 to 6.5 mass %, and even more preferably 0.8 to 5.0 mass %. This is from the viewpoint of obtaining a coating film excellent in metallic luster from the glitter coating composition.
- the solid content of the scale-like aluminum pigment (A) is preferably 30 to 200 parts by weight, more preferably 32 to 150 parts by weight, and even more preferably 35 to 100 parts by weight. This is from the viewpoint of obtaining a coating film excellent in metallic luster from the glitter coating composition.
- Nanocellulose (B) preferably contains at least one selected from cellulose nanofibers (B1) and cellulose nanocrystals (B2), and is more preferably cellulose nanofibers (B1). This is because the coating film formed from the glitter coating composition has excellent metallic luster. Further, when the glitter coating composition is applied using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, the glitter coating composition The composition has excellent ejection stability.
- Nanocellulose (B) is cellulose obtained by disentangling cellulose fibers to the nano-size level (defibration treatment).
- the cellulose fibers include natural cellulose fibers, regenerated cellulose fibers, semi-synthetic cellulose fibers, and modified cellulose fibers.
- the above natural cellulose fibers are obtained by removing impurities through a refining process from substances containing naturally occurring cellulose fibers.
- natural cellulose fiber-containing materials include woody materials such as conifers and hardwoods, cotton such as cotton linters and cotton lints, pomace such as sugar cane and sugar radish, bast fibers such as flax, ramie, jute and kenaf, and sisal. and leaf vein fiber such as pineapple, petiole fiber such as abaca and banana, fruit fiber such as coconut palm, stem fiber such as bamboo, bacterial cellulose produced by bacteria, seaweed such as valonia and cladophora, and cyst of sea squirt. .
- the regenerated cellulose fibers include rayon and cupra.
- semisynthetic cellulose fiber acetate etc. are mentioned, for example.
- modified cellulose fiber those obtained by chemically modifying cellulose can be used. Types of chemical modification include, for example, carboxymethylation, acylation, esterification such as phosphorylation, oxidation such as carboxylation, sulfonation, fluorination, cationization, and treatment with a silane coupling agent.
- the nanocellulose (B) may be chemically modified after being defibrated.
- nanocellulose (B) may be neutralized with a neutralizing agent.
- Neutralization with such a neutralizing agent improves the waterproof adhesion of nanocellulose (B) including cellulose nanofibers.
- the neutralizing agent is an organic base that is bulkier than an inorganic metal base such as sodium hydroxide. can be a neutralizing agent.
- Examples of preferred neutralizing agents include organic bases such as quaternary ammonium salts and amines (primary amines, secondary amines, tertiary amines).
- Preferred quaternary ammonium salts are quaternary ammonium hydroxides.
- Examples of the amines include alkylamines and alcoholamines. Examples of the alkylamine include N-butylamine, N-octylamine, dibutylamine, triethylamine and the like.
- Examples of the alcohol amine include N-butylethanolamine, N-methylethanolamine, 2-amino-2-methyl-1-propanol, dimethylethanolamine, dibutylethanolamine, and methyldiethanolamine.
- the content of the neutralizing agent is not particularly limited as long as it is an amount that can neutralize part or all of the oxidized cellulose, but the neutralization equivalent to the acid groups contained is preferably 0.2 to 1.0 equivalent.
- the number average fiber diameter of nanocellulose (B) is preferably within the range of 1 to 500 nm. Also, the number average length of nanocellulose (B) is preferably in the range of 10 to 10,000 nm.
- the number average fiber diameter and number average length of nanocellulose (B) can be examined by SEM analysis. For example, 50 nanocellulose (B) fibers can be examined and the average value can be calculated.
- the aspect ratio which is the ratio of the number average length of the nanocellulose (B) to the number average fiber diameter (number average length/number average fiber diameter), is the metallic luster of the coating film formed from the glitter coating composition. From the viewpoint of ejection stability of the glitter coating composition, etc., it is preferably in the range of 3 to 10,000, more preferably in the range of 5 to 500.
- the cellulose nanofiber (B1) has an aspect ratio of 50 or more.
- the cellulose nanocrystal (B2) has an aspect ratio of less than 50.
- Cellulose nanofibers (B1) can be obtained by a known method.
- cellulose nanofibers (B1) can be obtained by subjecting a cellulose raw material to a fibrillation treatment to reduce the fiber diameter to nanosize.
- the defibration treatment method for the cellulose raw material include mechanical fibrillation treatment and chemical treatment such as treatment with an oxidation catalyst solution containing an N-oxyl compound.
- the cellulose raw material is not particularly limited as long as it contains cellulose, but examples include various wood pulps, non-wood pulps, bacterial cellulose, regenerated cellulose, waste paper pulp, cotton, valonia cellulose, sea squirt cellulose, and the like. Also, various commercially available cellulose powders and microcrystalline cellulose powders may be used.
- cellulose nanofibers (B1) that have undergone various chemical modifications can be used.
- Types of chemical modification include, for example, carboxymethylation, acylation, esterification such as phosphorylation, oxidation such as carboxylation, sulfonation, fluorination, cationization, and treatment with a silane coupling agent.
- the cellulose nanofibers (B1) may be neutralized with a neutralizing agent.
- the neutralizing agent for example, the neutralizing agent described in the explanation column of the nanocellulose (B) can be used.
- the number average fiber diameter of the cellulose nanofibers (B1) is in the range of 1 to 500 nm from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. preferably within the range of 1 to 250 nm, particularly preferably within the range of 2 to 50 nm.
- the number average length of the cellulose nanofibers (B1) is in the range of 200 to 10,000 nm from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. preferably within the range of 200 to 5,000 nm, particularly preferably within the range of 300 to 2,500 nm, and further preferably within the range of 200 to 1,000 nm. Especially preferred.
- the aspect ratio of the cellulose nanofibers (B1) is in the range of 50 to 500 from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. more preferably in the range of 50-200, and particularly preferably in the range of 50-150.
- Examples of commercially available cellulose nanofibers (B1) include “Nanocellulose Fiber” (manufactured by Chuetsu Pulp Co., Ltd.), “BiNFi-s” (manufactured by Sugino Machine Co., Ltd.), and “Rheocrysta” (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.). , “Cellulose Nanofiber” (manufactured by Mori Machinery Co., Ltd.), “Serenpia” (manufactured by Nippon Paper Industries Co., Ltd.), “Auro Visco” (manufactured by Oji Holding Co., Ltd.), and the like.
- Cellulose nanocrystals (B2) can be obtained by a known method.
- Cellulose nanocrystals (D2) can be obtained, for example, by treating a cellulose raw material with an acid such as sulfuric acid to hydrolyze and remove non-crystalline portions, followed by mechanical fibrillation.
- the cellulose raw material is not particularly limited as long as it contains cellulose, and the same cellulose raw material as the cellulose nanofiber (B1) raw material can be used.
- the mechanical fibrillation treatment is also not particularly limited, and conventionally known methods such as high-pressure homogenizers, ultra-high-pressure homogenizers, ball mills, roll mills, cutter mills, planetary mills, jet mills, attritors, grinders, juicer mixers, and homomixers. , an ultrasonic homogenizer, a nanogenizer, underwater counter-impingement, a method using a single-screw or twin-screw extruder, or the like can be used.
- various chemically modified cellulose nanocrystals can be used.
- Types of chemical modification include, for example, carboxymethylation, acylation, esterification such as phosphorylation, oxidation such as carboxylation, sulfonation, fluorination, cationization, and treatment with a silane coupling agent.
- the cellulose nanocrystals (B2) may be neutralized with a neutralizing agent.
- a neutralizing agent for example, the neutralizing agent described in the section on nanocellulose (B) can be used.
- the number average fiber diameter of the cellulose nanocrystals (B2) is in the range of 1 to 50 nm from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. preferably within the range of 1 to 30 nm, particularly preferably within the range of 1 to 15 nm, and even more preferably within the range of 1 to 5 nm.
- the number average length of the cellulose nanocrystals (B2) is 10 to 500 nm from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. It is preferably within the range, more preferably within the range of 10 to 300 nm, particularly preferably within the range of 20 to 250 nm, and even more preferably within the range of 30 to 150 nm.
- the aspect ratio of the cellulose nanocrystals (B2) is 3 or more and less than 50 from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like. is preferred, 5 or more and less than 50 is more preferred, and 10 or more and less than 50 is even more particularly preferred.
- Examples of commercially available cellulose nanocrystals (B2) include "Celluforce NCC" (manufactured by Celluforce).
- the solid content of nanocellulose (B) is 5 to 60 parts by mass with respect to the total 100 parts by mass of the solid content of the components excluding the scale-like aluminum pigment (A). parts by mass, more preferably 10 to 50 parts by mass, even more preferably 15 to 40 parts by mass. This is from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition, the ejection stability of the glitter coating composition, and the like.
- nanocellulose (B) is added to the entire glitter coating composition. Based on the mass, the content is preferably in the range of 0.1 to 1.7 mass %, more preferably 0.4 to 1.3 mass %, and even more preferably 0.45 to 1.1 mass %.
- the glitter coating composition can further contain a resin, and examples of the resin include acrylic resin (C), polyester resin, alkyd resin, polyurethane resin, epoxy resin, silicone resin, and any combination thereof. It is preferably an acrylic resin (C). This is from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition.
- the phosphoric acid group-containing resin is included in the phosphoric acid group-containing compound (D) described below.
- the above resin is preferably an emulsion, for example, an acrylic resin emulsion, a polyester resin emulsion, an alkyd resin emulsion, a polyurethane resin emulsion, an epoxy resin emulsion, a silicone resin emulsion, any combination thereof, and the like, and an acrylic resin.
- Emulsions are preferred. This is from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition.
- the acrylic resin (C) is preferably a hydroxyl group-containing acrylic resin having at least one hydroxyl group in one molecule.
- a known water-soluble or water-dispersible hydroxyl group-containing acrylic resin that has been conventionally used in water-based paints can be used.
- the hydroxyl group-containing acrylic resin (C') is obtained by, for example, using a hydroxyl group-containing polymerizable unsaturated monomer and another polymerizable unsaturated monomer copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer by a method known per se, such as It can be produced by copolymerization by a method such as solution polymerization.
- the hydroxyl group-containing polymerizable unsaturated monomer is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated bonds in one molecule, for example, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl Monoesterified product of glycol such as meth)acrylate and polyethylene glycol mono(meth)acrylate and acrylic acid or methacrylic acid; ring-opening polymerization of ⁇ -caprolactone to the monoesterified product of polyhydric alcohol and acrylic acid or methacrylic acid; compound and the like.
- polymerizable unsaturated monomers copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer can be appropriately selected and used according to the properties desired for the hydroxyl group-containing acrylic resin (C'). Specific examples of the monomers are listed below. These can be used alone or in combination of two or more.
- (meth)acrylate means acrylate or methacrylate.
- (Meth)acrylic acid means acrylic acid or methacrylic acid.
- (meth)acryloyl means acryloyl or methacryloyl.
- (Meth)acrylamide means acrylamide or methacrylamide.
- alkyl or cycloalkyl (meth)acrylates for example methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-Butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate acrylates, tridecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl
- a polymerizable unsaturated monomer having an isobornyl group such as isobornyl (meth)acrylate
- Polymerizable unsaturated monomers having an adamantyl group such as adamantyl (meth)acrylate.
- Polymerizable unsaturated monomers having a tricyclodecenyl group such as tricyclodecenyl (meth)acrylate.
- Aromatic ring-containing polymerizable unsaturated monomers for example, benzyl (meth)acrylate, styrene, ⁇ -methylstyrene, vinyltoluene and the like.
- polymerizable unsaturated monomers having an alkoxysilyl group for example, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, ⁇ -(meth)acryloyloxypropyltrimethoxysilane, ⁇ -( meth)acryloyloxypropyltriethoxysilane and the like.
- polymerizable unsaturated monomers having a fluorinated alkyl group perfluoroalkyl (meth)acrylates such as perfluorobutylethyl (meth)acrylate and perfluorooctylethyl (meth)acrylate; fluoroolefins and the like.
- Vinyl compounds for example, N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, vinyl acetate and the like.
- phosphoric acid group-containing polymerizable unsaturated monomers for example, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 2-acryloyloxypropyl acid phosphate, 2-methacryloyloxypropyl acid phosphate and the like.
- (xi) carboxyl group-containing polymerizable unsaturated monomers for example, (meth)acrylic acid, maleic acid, crotonic acid, ⁇ -carboxyethyl acrylate and the like;
- (xii) nitrogen-containing polymerizable unsaturated monomers for example, (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N- dimethylaminopropyl(meth)acrylamide, methylenebis(meth)acrylamide, ethylenebis(meth)acrylamide, 2-(methacryloyloxy)ethyltrimethylammonium chloride, adducts of glycidyl(meth)acrylate and amines, and the like.
- (xiii) Polymerizable unsaturated monomers having at least two polymerizable unsaturated groups per molecule: for example, allyl (meth)acrylate, 1,6-hexanediol di(meth)acrylate and the like.
- epoxy group-containing polymerizable unsaturated monomers for example, glycidyl (meth)acrylate, ⁇ -methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate ) acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, allyl glycidyl ether and the like.
- polymerizable unsaturated monomers having a sulfonic acid group for example, 2-acrylamido-2-methylpropanesulfonic acid, 2-sulfoethyl (meth)acrylate, allylsulfonic acid, 4-styrenesulfonic acid; sodium salts and ammonium salts and the like.
- UV-absorbing functional groups such as 2-hydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2-hydroxy-4-(3-acryloyloxy-2 -hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2-(2'
- photostable polymerizable unsaturated monomers for example 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyloxy-2,2,6, 6-tetramethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6 ,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6, 6-tetramethylpiperidine, 4-crotonoylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine and the like.
- the hydroxyl group-containing acrylic resin (C') preferably has a hydroxyl value of 10 to 150 mgKOH/g, more preferably 15 to 100 mgKOH/g.
- the hydroxyl group-containing acrylic resin (C') preferably has an acid value of 150 mgKOH/g or less, more preferably 145 mgKOH/g or less.
- the hydroxyl group-containing acrylic resin (C') preferably has a weight average molecular weight of 1,000 to 100,000, more preferably 2,000 to 60,000.
- the weight average molecular weight of the hydroxyl group-containing acrylic resin (C′) is the retention time (retention capacity) measured using gel permeation chromatography (GPC) under the same conditions. It is a value obtained by converting the retention time (retention volume) of standard polystyrene into the molecular weight of polystyrene.
- GPC gel permeation chromatography
- the glitter coating composition of the present disclosure contains an acrylic resin (C) in an amount of 0.1 to 20% by mass based on the total weight of the glitter coating composition in order to obtain a coating film with excellent metallic gloss. It is preferably contained within the range, more preferably within the range of 0.3 to 10% by mass, and further preferably within the range of 0.45 to 5% by mass.
- the solid content of the acrylic resin (C) is 10 to 70 parts by mass with respect to the total 100 parts by mass of the solid content of the components excluding the scale-like aluminum pigment (A). parts by mass, more preferably 15 to 65 parts by mass, even more preferably 20 to 60 parts by mass. This is from the viewpoint of obtaining a coating film excellent in metallic luster.
- the glitter coating composition preferably further contains a phosphoric acid group-containing compound (D).
- D phosphoric acid group-containing compound
- the coating film formed from the glitter coating composition tends to have excellent metallic luster.
- the glitter coating composition is applied using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, the glitter coating composition The composition has excellent ejection stability.
- Phosphate group-containing compounds (D) include, for example, phosphoric acid; mono-n-propyl phosphate, monoisopropyl phosphate, mono-n-butyl phosphate, monoisobutyl phosphate, mono-tert-butyl phosphate, monooctyl phosphoric acid, monoalkyl phosphate such as monodecyl phosphate; di-n-propyl phosphate, diisopropyl phosphate, di-n-butyl phosphate, diisobutyl phosphate, di-tert-butyl phosphate, dioctyl phosphate, didecyl phosphate Dialkyl phosphate; mono-n-propyl phosphite, monoisopropyl phosphite, mono-n-butyl phosphite, monoisobutyl phosphite, mono-tert-butyl phosphite,
- a phosphate group-containing resin and a phosphate ester are preferred.
- the phosphoric acid group-containing resin is preferable from the viewpoint of water resistance, chipping resistance, etc., and the phosphate ester is useful for the storage stability of the glitter coating composition and the coating film formed from the glitter coating composition. It is preferable from the viewpoint of metallic luster.
- phosphoric acid group-containing resins examples include phosphoric acid group-containing acrylic resins, phosphoric acid group-containing polyester resins, phosphoric acid group-containing polyether resins, phosphoric acid group-containing polycarbonate resins, phosphoric acid group-containing polyurethane resins, and phosphoric acid group-containing epoxy resins. Resins and the like can be mentioned, and phosphate group-containing acrylic resins are preferable. This is from the viewpoint of the water resistance and chipping resistance of the coating film formed from the glitter coating composition.
- the phosphoric acid group-containing acrylic resin can be synthesized by copolymerizing a polymerizable unsaturated monomer having a phosphoric acid group and other polymerizable unsaturated monomers by a conventional method.
- Polymerizable unsaturated monomers having a phosphoric acid group include polymerizable unsaturated monomers having a phosphoric acid group: acid phosphooxyethyl (meth)acrylate, acid phosphooxypropyl (meth)acrylate, acid phosphooxypoly(oxyethylene) Glycol (meth)acrylate, acid phosphooxypoly(oxypropylene)glycol (meth)acrylate and the like.
- the polymerizable unsaturated monomer having a phosphoric acid group is 1 to 50 mass%, particularly 5 to 40 mass%, based on the total amount of each monomer component constituting the phosphoric acid group-containing acrylic resin. % is preferred.
- the phosphate group-containing acrylic resin preferably has a 000 range of weight average molecular weight.
- the solid content of the phosphoric acid group-containing compound (D) is 10 parts per 100 parts by mass of the total solid content of the components excluding the scale-like aluminum pigment (A). It is preferably in the range of up to 60 parts by mass, more preferably in the range of 15 to 55 parts by mass, and even more preferably in the range of 20 to 50 parts by mass.
- the glitter coating composition of the present disclosure contains a phosphoric acid group-containing compound (D) of preferably 0.1 to 1.7% by mass, more preferably 0.4%, based on the total mass of the glitter coating composition. ⁇ 1.3 wt%, and more preferably in the range of 0.45 to 1.1 wt%.
- the phosphate group-containing compound (D) is a phosphate group-containing acrylic resin
- the phosphate group-containing acrylic resin is not included in the acrylic resin (C).
- the glitter coating composition may further contain a curing agent capable of reacting with the resin.
- the curing agent include amino resins, polyisocyanate compounds, blocked polyisocyanate compounds, epoxy group-containing compounds, carboxyl group-containing compounds, carbodiimide group-containing compounds, hydrazide group-containing compounds, semicarbazide group-containing compounds, and the like.
- amino resins capable of reacting with hydroxyl groups, polyisocyanate compounds and blocked polyisocyanate compounds, and compounds containing carbodiimide groups capable of reacting with carboxyl groups are preferred.
- the bright coating composition preferably has a solid content concentration of 1.0 to 15.0% by mass, more preferably 1.5 to 10.0% by mass, and even more preferably 2.0 to 8.0% by mass. have This is from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition and the resistance to occurrence of unevenness.
- the glitter coating composition has excellent coating stability when applied, and the glitter coating composition controls ejection by changing the relative distance between the valve body and the ejection port. In the case of coating using a liquid ejection head, the glitter coating composition is excellent in ejection stability.
- the solid content concentration is measured at 110 ° C. after weighing the measurement object (e.g., glitter paint composition) into a heat-resistant container such as an aluminum foil cup and spreading the measurement object on the bottom of the container. Drying for 1 hour, weighing the mass of the components in the measurement object remaining after drying, and obtaining the ratio of the mass of the component in the measurement object remaining after drying to the total mass of the measurement object before drying It can be calculated by
- the above-mentioned glitter coating composition may optionally contain organic solvents, thickeners, curing catalysts, ultraviolet absorbers, light stabilizers, antifoaming agents, plasticizers, surface conditioners, anti-settling agents, etc. for various coatings. Additives can be included.
- the glitter coating composition of the present disclosure can be applied by a method known in the art without any particular limitation. can be coated with As a result, the glitter coating composition has excellent ejection stability when applied using a liquid ejection head.
- the luster coating composition is produced by shortening the relative distance between the valve body and the ejection port.
- Examples include those that discharge, and those that discharge the glitter coating composition by increasing the relative distance between the valve body and the discharge port.
- liquid ejection head examples include an on-demand type (for example, a piezo type, a thermal type, a valve type), a continuous type, and the like, and an on-demand type, particularly a piezo type, is preferable. This is because the ejection property of the high-viscosity glitter coating composition is excellent.
- the piezo-type liquid ejection head examples include piezo jet dispenser manufactured by SSI JAPAN Co., Ltd., X JET (model for high viscosity liquid), and the like.
- the multilayer coating film forming method of the present disclosure includes the following steps. Step 1: Using a liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port, the above-described Step of forming a glitter coating film on the object to be coated ⁇ Step 2: A step of applying a clear coating composition to the glitter coating film to form a clear coating film
- the liquid ejection head that controls ejection by changing the relative distance between the valve body and the ejection port is as described in the "Glitter Coating Composition" section.
- the dry film thickness of the glitter coating film formed from the glitter coating composition varies depending on the application of the article to be coated and is not particularly limited, but is preferably 0.5 to 2.0 ⁇ m, more preferably 0.7 to 0.7 ⁇ m. 1.8 ⁇ m, and more preferably 0.8-1.5 ⁇ m. This is from the viewpoint of the metallic luster of the coating film formed from the glitter coating composition and the resistance to occurrence of unevenness.
- Examples of the object to be coated include the outer plate of automobile bodies such as passenger cars, trucks, motorcycles, and buses; automobile parts; the outer plate of home electric appliances such as mobile phones and audio equipment. Skin parts and automotive parts are preferred.
- the material to be coated is not particularly limited, and examples thereof include iron, aluminum, brass, copper, tinplate, stainless steel, galvanized steel, zinc alloys (Zn-Al, Zn-Ni, Zn-Fe etc.) metal materials such as plated steel; resins such as polyethylene resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, epoxy resin, Plastic materials such as fiber reinforced plastics (FRP); inorganic materials such as glass, cement and concrete; wood; fiber materials such as paper and cloth.
- resins such as polyethylene resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, epoxy resin, Plastic materials such as fiber reinforced plastics (FRP); inorganic materials such as glass, cement
- the surface of the object to be coated may be a metal surface such as an outer plate of an automobile body, an automobile part, a home electric appliance, or a metal substrate such as a steel plate that constitutes these.
- Surface treatment such as treatment may be applied.
- a coating film may be further formed on objects that may or may not be surface-treated.
- an article to be coated which is a substrate, may be surface-treated as necessary, and an undercoat film may be formed thereon, or an intermediate paint film may be formed on the undercoat film.
- the primer coating film and the intermediate coating film can be formed using known primer and intermediate coating paints that are commonly used in the coating of automobile bodies. can.
- the above-mentioned proximity discharge is not particularly limited as long as the distance between the discharge port and the object to be coated is generally used in the above-described liquid discharge head, and is preferably 0.1 to 50.0 mm, more preferably 0 .5 to 30.0 mm, and more preferably 1.0 to 10.0 mm.
- the frequency when ejecting the glitter coating composition from the valve body is 10 to 10,000 Hz from the viewpoint of ejection stability and difficulty in causing unevenness in the formed coating film. is preferably within the range of , more preferably within the range of 30 to 5,000 Hz, and even more preferably within the range of 50 to 3,000 Hz.
- the supply pressure for supplying the glitter coating composition to the liquid ejection head is preferably in the range of 0.001 to 10 MPa from the viewpoint of supply stability, etc., and 0.005 It is more preferably in the range of ⁇ 5.0 MPa, more preferably in the range of 0.01 to 1.0 MPa.
- the scanning speed of the liquid ejection head should be in the range of 10 to 1,500 mm/s from the viewpoint of ejection stability and difficulty in causing unevenness in the formed coating film. , more preferably in the range of 50 to 1,000 mm/s, and even more preferably in the range of 100 to 800 mm/s.
- the pitch at which the liquid ejection head is scanned is preferably in the range of 0.001 to 1.0 mm, more preferably 0.005 to 1.0 mm, from the viewpoint of coating efficiency. more preferably within the range of 0.01 to 1.0 mm.
- the clear coating composition examples include curable clear coating compositions (eg, thermosetting clear coating compositions, photocurable clear coating compositions) and non-curable clear coating compositions.
- examples of the thermosetting clear coating composition include an organic solvent type thermosetting coating composition containing a base resin having a crosslinkable functional group and a curing agent, a water-based thermosetting coating composition, and a powder thermosetting coating composition.
- a paint composition etc. can be mentioned.
- Examples of crosslinkable functional groups possessed by the base resin include carboxyl groups, hydroxyl groups, epoxy groups, and silanol groups.
- Examples of types of base resins include acrylic resins, polyester resins, alkyd resins, urethane resins, epoxy resins, and fluorine resins.
- Examples of curing agents include polyisocyanate compounds, blocked polyisocyanate compounds, melamine resins, urea resins, carboxyl group-containing compounds, carboxyl group-containing resins, epoxy group-containing resins, and epoxy group-containing compounds.
- Combinations of base resin/curing agent for the clear coating composition include hydroxyl group-containing resin/polyisocyanate compound, carboxyl group-containing resin/epoxy group-containing resin, hydroxyl group-containing resin/blocked polyisocyanate compound, and hydroxyl group-containing resin/melamine resin. etc. are preferred, and a hydroxyl group-containing resin/polyisocyanate compound is more preferred.
- the clear coating composition may be a one-component coating or a multi-component coating such as a two-component urethane resin coating.
- the above clear coating composition may contain, if necessary, coloring pigments, luster pigments, dyes, etc., to such an extent that transparency is not hindered. Defoamers, thickeners, rust inhibitors, surface conditioners and the like can be contained as appropriate.
- the coating method of the clear coating composition is not particularly limited, but for example, a wet coating film can be formed by a coating method such as air spray coating, airless spray coating, rotary atomization coating, or curtain coating. In these coating methods, static electricity may be applied as necessary. Among them, air spray coating or rotary atomization coating is particularly preferable.
- the coating amount of the clear coating composition is generally such that the cured film thickness is 10 to 70 ⁇ m, preferably 20 to 50 ⁇ m.
- the present disclosure will be described more specifically with production examples, examples, and comparative examples. However, the present disclosure is not limited by these. In each example, “parts” and “%” are based on mass unless otherwise specified. Moreover, the film thickness of the coating film is based on the cured coating film.
- the remaining monomer emulsion (1) was added dropwise over 3 hours into the reaction vessel maintained at the same temperature, and after completion of the dropwise addition, aging was performed for 1 hour.
- the following monomer emulsion (2) was added dropwise over 1 hour, and after aging for 1 hour, 40 parts of a 5% dimethylethanolamine aqueous solution was gradually added to the reaction vessel while cooling to 30 ° C., and a 100-mesh nylon was prepared.
- the mixture was discharged while being filtered through a cloth to obtain an acrylic resin (C-1) emulsion having a solid concentration of 30%.
- the obtained acrylic resin (C-1) emulsion had an acid value of 33 mgKOH/g and a hydroxyl value of 25 mgKOH/g.
- Monomer emulsion (1) 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2.1 parts of methylenebisacrylamide, 2.8 parts of styrene, 16.1 parts of methyl methacrylate, 28 parts of ethyl acrylate and 21 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).
- Monomer emulsion (2) 18 parts of deionized water, 0.31 parts of "Aqualon KH-10", 0.03 parts of ammonium persulfate, 5.1 parts of methacrylic acid, 5.1 parts of 2-hydroxyethyl acrylate, 3 parts of styrene , 6 parts of methyl methacrylate, 1.8 parts of ethyl acrylate and 9 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (2).
- the following monomer emulsion (4) was added dropwise over 1 hour, and after aging for 1 hour, 40 parts of a 5% dimethylethanolamine aqueous solution was gradually added to the reaction vessel while cooling to 30 ° C., and 100 mesh nylon. The mixture was discharged while being filtered through cloth to obtain an acrylic resin (C-2) emulsion having a solid concentration of 30%.
- the obtained acrylic resin (C-2) emulsion had an acid value of 13 mgKOH/g and a hydroxyl value of 65 mgKOH/g.
- Monomer emulsion (3) 46.2 parts of deionized water, 0.79 parts of "Aqualon KH-10", 7.7 parts of styrene, 16.94 parts of methyl methacrylate, 7.7 parts of n-butyl acrylate, n- 30.8 parts of butyl methacrylate, 11.55 parts of 2-hydroxyethyl methacrylate and 2.31 parts of ethylene glycol dimethacrylate were mixed and stirred to obtain a monomer emulsion (3).
- Monomer emulsion (4) 13.8 parts of deionized water, 0.24 parts of "Aqualon KH-10", 0.03 parts of ammonium persulfate, 2.3 parts of styrene, 6.9 parts of methyl methacrylate, 4 parts of ethyl acrylate. 6 parts, 3.68 parts of n-butyl acrylate, 3.45 parts of 2-hydroxyethyl methacrylate and 2.07 parts of methacrylic acid were mixed and stirred to obtain a monomer emulsion (4).
- the obtained acrylic resin (D-1) solution having a solid content of 50% and having a hydroxyl group and a phosphoric acid group.
- the obtained acrylic resin (D-1) having a hydroxyl group and a phosphoric acid group had an acid value of 83 mgKOH/g, a hydroxyl value of 29 mgKOH/g and a weight average molecular weight of 10,000.
- Phosphate group-containing polymerizable monomer 57.5 parts of monobutyl phosphate and 41.0 parts of isobutanol are placed in a reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, nitrogen inlet tube and dropping device, and the temperature is adjusted to 90°C. After the temperature was raised to , 42.5 parts of glycidyl methacrylate was added dropwise over 2 hours, and the mixture was further stirred and aged for 1 hour. Then, 59.0 parts of isopropanol was added to obtain a phosphate group-containing polymerizable monomer solution having a solid concentration of 50%. The acid value of the obtained monomer was 285 mgKOH/g.
- Glitter coating composition No. 1 was prepared in the same manner as in Example 1, except that the formulation composition was changed to that shown in Table 2 below. 2 to No. 22 was obtained.
- Glitter coating composition No. 1 to No. 22 was filled in "X JET” (trade name, manufactured by SSI JAPAN Co., Ltd., high-viscosity micro-volume piezo jet dispenser, discharge port diameter 100 ⁇ m).
- the glitter coating composition No. 1 was applied to the object to be coated under the conditions of a frequency of 350 Hz, a supply pressure of 0.03 MPa, a speed of 230 mm/s, and a distance between the discharge port and the object to be coated of 10 mm. 1 to No.
- Each of No. 22 was applied in a linear shape (10 cm in length), and the distortion of the linear object was observed and evaluated. ⁇ and 0 are acceptable. Table 2 shows the evaluation results.
- ⁇ There is no distortion in the linear object.
- Good The linear material is partially distorted, but there is no practical problem.
- ⁇ There is a distortion in the linear product as a whole, and there is a problem in practical use.
- x A linear product cannot be formed.
- A There is no variation in the discharge amount of the glitter coating composition.
- ⁇ Slight variation in the discharge amount of the glitter coating composition, but no practical problem.
- ⁇ The discharge amount of the glitter coating composition varies greatly, and there is a problem in practical use.
- x Discharge of the glitter coating composition is not possible.
- [Preparation of coated object for flip-flop test and unevenness test] [Preparation of coated object (O-1) for flip-flop test and unevenness test] The surface of a black polypropylene plate measuring 100 mm long, 100 mm wide, and 2 mm thick was wiped with a gauze impregnated with petroleum benzine for degreasing, and then coated with "Ascarex #2850" (trade name, manufactured by Kansai Paint Co., Ltd.). Polyolefin-containing water-based primer paint) was applied with a hand spray gun so that the cured coating film was 15 ⁇ m, allowed to stand for 5 minutes, and then preheated at 80° C. for 3 minutes. Next, after standing for 7 minutes, the substrate was heated at 80° C. for 30 minutes to cure the primer coating film, thereby preparing an article to be coated (O-1).
- Electrodeposition coating was performed so as to have a thickness of 20 ⁇ m, and the coating was cured by heating at 170° C. for 30 minutes to form an electrodeposition coating film.
- Electrodeposition coating was performed so as to have a thickness of 20 ⁇ m, and the coating was cured by heating at 170° C. for 30 minutes to form an electrodeposition coating film.
- the clear coating composition (Z-1) obtained in Production Example 17 was applied to the uncured glitter coating film with a hand spray gun so that the cured film thickness was 35 ⁇ m, left for 7 minutes, and heated to 80°C.
- a coated plate (S1-1) was prepared by heating for 30 minutes to cure the coating film.
- Glitter coating composition No. 1 is filled into “X JET” (trade name, SSI JAPAN Co., Ltd., high-viscosity micro-volume piezo jet dispenser, discharge port diameter 100 ⁇ m), and the object to be coated (O-4) is applied with a frequency of 350 Hz, a supply pressure of 0.03 MPa, a pitch 1 mm, the distance between the outlet and the object to be coated is 10 mm, the conditions are 23 ° C. and 68% relative humidity, and the dry film thickness is 1 ⁇ m. After leaving it at room temperature for 5 minutes, preheat at 80 ° C. for 3 minutes. to form an uncured glitter coating film.
- Glitter coating composition No. 1 was applied to the object to be coated (O-5). 1 is applied using a robot bell manufactured by ABB under the conditions of 23 ° C. and 68% relative humidity so that the dry film thickness is 1 ⁇ m, left at room temperature for 5 minutes, and then preheated at 80 ° C. for 3 minutes. to form an uncured glitter coating film.
- Example 18 to 36 and Comparative Examples 7 to 12 A coated plate (S1 -21) ⁇ (S1-26), (S2-2) ⁇ (S2-26), (S3-2) ⁇ (S3-26), (S4-2) ⁇ (S4-26), (S5-2 ) to (S5-26) and (S6-2) to (S6-26) were produced.
- (S1-21) ⁇ (S1-23), (S2-21) ⁇ (S2-23), (S3-21) ⁇ (S3-23), (S4-21) ⁇ (S4-23) and (S5-21) to (S5-23) were not evaluated because the nozzle was clogged and coating was impossible.
Landscapes
- Chemical & Material Sciences (AREA)
- Life Sciences & Earth Sciences (AREA)
- Engineering & Computer Science (AREA)
- Wood Science & Technology (AREA)
- Organic Chemistry (AREA)
- Materials Engineering (AREA)
- Inorganic Chemistry (AREA)
- Dispersion Chemistry (AREA)
- Paints Or Removers (AREA)
- Application Of Or Painting With Fluid Materials (AREA)
Priority Applications (4)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| EP22895413.7A EP4434639A4 (en) | 2021-11-18 | 2022-10-28 | Photoluminescent coating material composition and multilayer coating film forming method |
| US18/695,626 US20250122387A1 (en) | 2021-11-18 | 2022-10-28 | Photoluminescent coating material composition and multilayer coating film forming method |
| CN202280065240.2A CN118043414A (zh) | 2021-11-18 | 2022-10-28 | 光亮性涂料组合物和多层涂膜形成方法 |
| JP2023507349A JP7249476B1 (ja) | 2021-11-18 | 2022-10-28 | 光輝性塗料組成物、及び複層塗膜形成方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021188057 | 2021-11-18 | ||
| JP2021-188057 | 2021-11-18 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023090130A1 true WO2023090130A1 (ja) | 2023-05-25 |
Family
ID=86396825
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2022/040487 Ceased WO2023090130A1 (ja) | 2021-11-18 | 2022-10-28 | 光輝性塗料組成物、及び複層塗膜形成方法 |
Country Status (5)
| Country | Link |
|---|---|
| US (1) | US20250122387A1 (cg-RX-API-DMAC7.html) |
| EP (1) | EP4434639A4 (cg-RX-API-DMAC7.html) |
| JP (1) | JP7249476B1 (cg-RX-API-DMAC7.html) |
| CN (1) | CN118043414A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023090130A1 (cg-RX-API-DMAC7.html) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025150504A1 (ja) * | 2024-01-12 | 2025-07-17 | 関西ペイント株式会社 | 光輝性塗料組成物、塗膜形成方法及び複層塗膜形成方法 |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN117858928B (zh) * | 2021-09-13 | 2025-12-02 | 关西涂料株式会社 | 涂料组合物 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2011521093A (ja) * | 2008-05-28 | 2011-07-21 | エッカルト ゲゼルシャフト ミット ベシュレンクテル ハフツング | 添加剤を伴う金属効果顔料 |
| JP2012210764A (ja) | 2011-03-31 | 2012-11-01 | Fujifilm Corp | インクジェット記録方法及び印刷物 |
| JP2015193143A (ja) | 2014-03-31 | 2015-11-05 | 大日本塗料株式会社 | 加飾構造体及びその製造方法 |
| JP2017210553A (ja) * | 2016-05-25 | 2017-11-30 | 株式会社リコー | インク、インク収容容器、インクジェット方法、及びインクジェット装置 |
| WO2021172008A1 (ja) * | 2020-02-28 | 2021-09-02 | コニカミノルタ株式会社 | インクジェットインク及び画像形成方法 |
Family Cites Families (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP6386521B2 (ja) * | 2016-12-14 | 2018-09-05 | 大日本塗料株式会社 | メタリック塗料組成物 |
| JPWO2020044672A1 (ja) * | 2018-08-31 | 2021-09-09 | 関西ペイント株式会社 | 複層塗膜形成方法 |
| JP7519160B2 (ja) * | 2019-09-03 | 2024-07-19 | 関西ペイント株式会社 | 複層塗膜形成方法 |
-
2022
- 2022-10-28 EP EP22895413.7A patent/EP4434639A4/en active Pending
- 2022-10-28 CN CN202280065240.2A patent/CN118043414A/zh active Pending
- 2022-10-28 US US18/695,626 patent/US20250122387A1/en active Pending
- 2022-10-28 JP JP2023507349A patent/JP7249476B1/ja active Active
- 2022-10-28 WO PCT/JP2022/040487 patent/WO2023090130A1/ja not_active Ceased
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2011521093A (ja) * | 2008-05-28 | 2011-07-21 | エッカルト ゲゼルシャフト ミット ベシュレンクテル ハフツング | 添加剤を伴う金属効果顔料 |
| JP2012210764A (ja) | 2011-03-31 | 2012-11-01 | Fujifilm Corp | インクジェット記録方法及び印刷物 |
| JP2015193143A (ja) | 2014-03-31 | 2015-11-05 | 大日本塗料株式会社 | 加飾構造体及びその製造方法 |
| JP2017210553A (ja) * | 2016-05-25 | 2017-11-30 | 株式会社リコー | インク、インク収容容器、インクジェット方法、及びインクジェット装置 |
| WO2021172008A1 (ja) * | 2020-02-28 | 2021-09-02 | コニカミノルタ株式会社 | インクジェットインク及び画像形成方法 |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP4434639A4 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025150504A1 (ja) * | 2024-01-12 | 2025-07-17 | 関西ペイント株式会社 | 光輝性塗料組成物、塗膜形成方法及び複層塗膜形成方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| US20250122387A1 (en) | 2025-04-17 |
| CN118043414A (zh) | 2024-05-14 |
| JP7249476B1 (ja) | 2023-03-30 |
| EP4434639A4 (en) | 2026-03-04 |
| JPWO2023090130A1 (cg-RX-API-DMAC7.html) | 2023-05-25 |
| EP4434639A1 (en) | 2024-09-25 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7305545B2 (ja) | 複層塗膜形成方法 | |
| JP5430935B2 (ja) | 水性塗料組成物 | |
| JP7249476B1 (ja) | 光輝性塗料組成物、及び複層塗膜形成方法 | |
| JP6851329B2 (ja) | 光輝性顔料含有水性ベースコート塗料、及びこれを用いた複層塗膜形成方法 | |
| WO2008026767A1 (fr) | Composition de résine pour matériau de revêtement aqueux et composition de revêtement aqueux | |
| JP7519160B2 (ja) | 複層塗膜形成方法 | |
| JP3760028B2 (ja) | 複層塗膜形成法 | |
| CN112262189B (zh) | 水性涂料用表面调整剂、水性涂料组合物、涂膜以及多层涂膜 | |
| JP7757232B2 (ja) | 複層塗膜形成方法 | |
| US20250084259A1 (en) | Effect coating composition and method for forming multilayer coating film | |
| JP5757662B2 (ja) | 共重合体、該共重合体を含有する水性塗料組成物及び複層塗膜形成方法 | |
| CN115348902A (zh) | 多层涂膜的形成方法 | |
| JP4387503B2 (ja) | メタリック塗膜形成法 | |
| JP6654331B2 (ja) | 複層塗膜形成方法 | |
| US12515238B2 (en) | Method for forming multilayer coating film | |
| JP4020473B2 (ja) | メタリツク塗膜形成方法 | |
| JP7179419B2 (ja) | 塗膜形成方法 | |
| EP4695338A1 (en) | A waterborne coating composition and its applications thereof | |
| CN114345661B (zh) | 形成多层涂膜的方法 | |
| JP7397026B2 (ja) | 塗料組成物セット | |
| JP6696714B2 (ja) | クリヤーコート塗料、及びこれを用いた複層塗膜形成方法 | |
| JP5665132B2 (ja) | 共重合体、該共重合体を含有する水性塗料組成物及び複層塗膜形成方法 | |
| JP3999864B2 (ja) | メタリック塗膜形成方法 | |
| WO2023219117A1 (ja) | 複層塗膜製造方法および複層塗膜 | |
| JP2018103082A (ja) | 複層塗膜形成方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023507349 Country of ref document: JP |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22895413 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 18695626 Country of ref document: US |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280065240.2 Country of ref document: CN |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2022895413 Country of ref document: EP |
|
| ENP | Entry into the national phase |
Ref document number: 2022895413 Country of ref document: EP Effective date: 20240618 |
|
| WWP | Wipo information: published in national office |
Ref document number: 18695626 Country of ref document: US |