WO2023074346A1 - 炭素材及びその製造方法と、二次電池及びその製造方法 - Google Patents

炭素材及びその製造方法と、二次電池及びその製造方法 Download PDF

Info

Publication number
WO2023074346A1
WO2023074346A1 PCT/JP2022/037832 JP2022037832W WO2023074346A1 WO 2023074346 A1 WO2023074346 A1 WO 2023074346A1 JP 2022037832 W JP2022037832 W JP 2022037832W WO 2023074346 A1 WO2023074346 A1 WO 2023074346A1
Authority
WO
WIPO (PCT)
Prior art keywords
carbon material
particles
less
negative electrode
carbon
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/037832
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
博明 吉田
聡 平原
信亨 石渡
寿子 近藤
隆人 湯浅
正和 横溝
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsubishi Chemical Corp
Original Assignee
Mitsubishi Chemical Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Chemical Corp filed Critical Mitsubishi Chemical Corp
Priority to CN202280071387.2A priority Critical patent/CN118159490A/zh
Priority to KR1020247009172A priority patent/KR20240087705A/ko
Priority to JP2023556283A priority patent/JPWO2023074346A1/ja
Priority to CA3233421A priority patent/CA3233421A1/en
Priority to EP22886676.0A priority patent/EP4424636A4/en
Publication of WO2023074346A1 publication Critical patent/WO2023074346A1/ja
Priority to US18/621,202 priority patent/US20240243286A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/58—Selection of substances as active materials, active masses, active liquids of inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy; of polyanionic structures, e.g. phosphates, silicates or borates
    • H01M4/583—Carbonaceous material, e.g. graphite-intercalation compounds or CFx
    • H01M4/587—Carbonaceous material, e.g. graphite-intercalation compounds or CFx for inserting or intercalating light metals
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
    • C01B32/00—Carbon; Compounds thereof
    • C01B32/20—Graphite
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/052—Li-accumulators
    • H01M10/0525—Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/058—Construction or manufacture
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
    • H01M4/133—Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/60—Particles characterised by their size
    • C01P2004/61—Micrometer sized, i.e. from 1-100 micrometer
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/80—Particles consisting of a mixture of two or more inorganic phases
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/11—Powder tap density
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/12—Surface area
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M2004/021—Physical characteristics, e.g. porosity, surface area
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M2004/026—Electrodes composed of, or comprising, active material characterised by the polarity
    • H01M2004/027—Negative electrodes
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E60/00—Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
    • Y02E60/10—Energy storage using batteries

Definitions

  • the present invention relates to a carbon material as a negative electrode active material for secondary batteries, which has excellent cycle characteristics and achieves both a high capacity retention rate and a low DCR retention rate even after 500 cycles, and a method for producing the same.
  • the present invention also relates to a secondary battery using this carbon material as a negative electrode active material and a method for manufacturing the same.
  • lithium ion secondary batteries which have higher energy densities and superior large-current charge/discharge characteristics than nickel-cadmium batteries and nickel-hydrogen batteries.
  • Graphite materials and amorphous carbon are often used as negative electrode materials for lithium-ion secondary batteries because of their cost and durability.
  • amorphous carbon materials have a small reversible capacity within the range of materials that can be put into practical use.
  • the density of the active material layer containing the negative electrode material is increased in order to increase the capacity, the irreversible charge/discharge capacity during the initial cycle increases due to material breakdown, and as a result, the capacity does not increase.
  • Patent Document 1 as a negative electrode material for a non-aqueous secondary battery, it is possible to provide a non-aqueous secondary battery in which the reaction with the electrolyte solution is more suppressed and the deterioration during cycling is less.
  • a negative electrode carbon material for a non-aqueous secondary battery that can obtain a high-capacity non-aqueous secondary battery with excellent charge-discharge rate characteristics with little gas generation, a non-aqueous secondary containing the following (A) and (B) Anode materials for batteries have been proposed.
  • Composite carbon material (A) obtained by coating the pressure-treated carbon material (a) with a carbonaceous material or a graphite material
  • a carbonaceous material or a graphite material One type selected from natural graphite (C), artificial graphite (D), coated graphite (E) obtained by coating a raw carbon material that has not been pressure-treated with a carbonaceous substance or a graphite substance, and amorphous carbon (F)
  • C natural graphite
  • D artificial graphite
  • coated graphite (E) obtained by coating a raw carbon material that has not been pressure-treated with a carbonaceous substance or a graphite substance
  • amorphous carbon F
  • An object of the present invention is to provide a carbon material that achieves both a high capacity retention rate and a low DCR retention rate even after 500 cycles, and a secondary battery using the same.
  • the present inventors have found that the specific surface area is 10 m 2 /g or less, the number of peaks in the particle size distribution obtained from flow particle image analysis is 2 or more, and the number of particles obtained from flow particle image analysis is No.
  • the gist of the present invention is as follows.
  • the number of peaks in the particle size distribution obtained from the flow type particle image analysis is 2 or more, the number of particles Ne calculated by the following formula (1) is 700 or more, and the specific surface area is 10 m 2 /g or less, a carbon material.
  • Ne No ⁇ F (1)
  • No (number) is the number of particles of the carbon material obtained from the flow particle image analysis.
  • F (%) is the carbon material having a particle size of less than 3 ⁇ m obtained from the flow particle image analysis. is the particle frequency of
  • Ne(A) is the number of particles of the carbon material (A) calculated by the following formula (2)
  • Ne(B) is the number of particles of the carbon material (B) calculated by the following formula (3).
  • Ne(A) No(A) ⁇ F(A) (2)
  • Ne(B) No(B) ⁇ F(B) (3)
  • Ne(A) is the number of particles of the carbon material (A) calculated by the following formula (2)
  • Ne(B) is the number of particles of the carbon material (B) calculated by the following formula (3).
  • Ne(A) No(A) ⁇ F(A) (2)
  • Ne(B) No(B) ⁇ F(B) (3)
  • a secondary battery comprising a positive electrode, a negative electrode and an electrolyte, the negative electrode includes a current collector and a negative electrode active material layer formed on the current collector; A secondary battery, wherein the negative electrode active material layer contains the carbon material according to any one of [1] to [13].
  • a method for manufacturing a secondary battery comprising a positive electrode, a negative electrode and an electrolyte comprising: A method for producing a secondary battery, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [1] to [13] to obtain the negative electrode.
  • the carbon material of the present invention it is possible to provide a secondary battery that has excellent cycle characteristics and achieves both a high capacity retention rate and a low DCR retention rate even after 500 cycles.
  • the number of peaks in the particle size distribution obtained by flow particle image analysis is 2 or more, and the number of particles Ne calculated by the following formula (1) is 700 or more, It is characterized by having a specific surface area of 10 m 2 /g or less.
  • Ne No ⁇ F (1) (In formula (1), No (number) is the number of particles of the carbon material obtained from the flow particle image analysis. F (%) is the carbon material having a particle size of less than 3 ⁇ m obtained from the flow particle image analysis. is the particle frequency of
  • the electrical contact between the particles may be weakened due to the expansion and contraction of the negative electrode active material particles during the cycle. This weakening of the electrical contact causes isolation and deactivation of some particles, leading to deterioration of cycle characteristics.
  • graphite with a particle size distribution peak number of 2 or more, a particle number Ne of 700 or more, and a specific surface area of 10 m 2 /g or less fine particles of less than 3 ⁇ m are present in the gaps between large particles. can enter and fully fill the space.
  • the electrical contact between the particles is maintained during the cycle, and the isolation and deactivation of the particles are suppressed, leading to an improvement in the cycle characteristics.
  • the isolation and deactivation of particles also contributes to the deterioration of the DCR retention rate, it is considered that the improvement of the electrical contact improves the DCR retention rate as well as the cycle capacity retention rate.
  • the number of particles Ne of the carbon material of the present invention is preferably 700 or more, more preferably 1000 or more, and even more preferably 1500 or more.
  • the particle number Ne is excessively large, the excessive increase in the specific surface area may cause deterioration in battery durability. 1 or less is more preferable, 20,000 or less is more preferable, 10,000 or less is particularly preferable, and 7,000 or less is particularly preferable.
  • the specific surface area of the carbon material of the present invention is 10 m 2 /g or less, preferably 6.0 m 2 /g or less, more preferably 4.0 m 2 /g or less from the viewpoint of battery durability. more preferred.
  • the specific surface area of the carbon material of the present invention is preferably 1 m 2 /g or more, more preferably 1.5 m 2 /g or more. It is more preferably 0 m 2 /g or more.
  • various specific surface areas are values measured by the BET method using nitrogen adsorption.
  • the average particle size of the carbon material of the present invention is preferably 4 ⁇ m or more, more preferably 7 ⁇ m or more, and even more preferably 8 ⁇ m or more.
  • the average particle diameter of the carbon material of the present invention is preferably 24 ⁇ m or less, more preferably 19 ⁇ m or less, from the viewpoint of ensuring electrical contact between particles.
  • various average particle diameters are volume average particle diameters (median diameter (d50)) measured from a volume-based particle size distribution measured by a laser diffraction method.
  • the tap density of the carbon material of the present invention is preferably 0.60 g/cm 3 or more, more preferably 0.95 g/cm 3 or more, and 1.05 g/cm 3 or more. cm 3 or more is more preferable.
  • the tap density of the carbon material of the present invention is preferably 1.80 g/cm 3 or less, more preferably 1.35 g/cm 3 or less, from the viewpoint of ensuring electrical contact between particles. It is more preferably 1.25 g/cm 3 or less.
  • various tap densities are obtained by filling a cylindrical tap cell with a diameter of 1.6 cm and a volume capacity of 20 cm 3 fully using a powder density measuring instrument, and then tapping with a stroke length of 10 mm 1000 times. The density is calculated from the volume and mass of the sample at that time.
  • At least one of the two or more peaks in the particle size distribution of the carbon material of the present invention preferably exists between 10 ⁇ m and 25 ⁇ m.
  • the presence of the peak in the range of 10 ⁇ m to 25 ⁇ m provides good contact with particles less than 3 ⁇ m. From this point of view, it is preferable that the carbon material of the present invention has one peak in the particle size distribution, particularly in the range of 10 ⁇ m to 25 ⁇ m.
  • At least one of the two or more peaks in the particle size distribution of the carbon material of the present invention preferably exists between 1 ⁇ m and 5 ⁇ m. Existence of the peak in the range of 1 ⁇ m to 5 ⁇ m provides good contact with particles of 10 ⁇ m to 25 ⁇ m. From this point of view, it is preferable that the carbon material of the present invention has one peak in the particle size distribution, particularly in the range of 1 ⁇ m to 5 ⁇ m.
  • a carbon material having two or more peaks in the particle size distribution can be produced by mixing two or more carbon materials having different numbers of particles.
  • both the peak number of the particle size distribution and the particle number Ne can be within the above ranges.
  • a carbon material having a volume average particle size of 12 ⁇ m to 25 ⁇ m and a carbon material having a volume average particle size of 5 ⁇ m to 11 ⁇ m are used as two or more kinds of carbon materials to be used.
  • the carbon material can have particle size distribution peaks at 25 ⁇ m and from 1 ⁇ m to 5 ⁇ m.
  • the number of peaks in the particle size distribution is the value measured from the particle size distribution measured by flow particle image analysis.
  • the carbon material of the present invention When the carbon material of the present invention is obtained by mixing two or more kinds of carbon materials having different numbers of particles, the carbon material of the present invention consists of a carbon material (A) with less Ne (A) and a carbon material with more Ne (B). From the standpoint of battery durability, it is preferable that the battery is manufactured by mixing the material (B).
  • Ne(A) is the number of particles of the carbon material (A) calculated by the following formula (2)
  • Ne(B) is the number of particles of the carbon material (B) calculated by the following formula (3). number.
  • No (A) (number) is the number of particles of the carbon material (A) obtained from the flow particle image analysis.
  • F(A) (%) is the particle frequency of the carbon material (A) having a particle size of less than 3 ⁇ m obtained from the flow particle image analysis.
  • No (B) (pieces) is the number of particles of the carbon material (B) obtained from flow particle image analysis.
  • F(B) (%) is the particle frequency of the carbon material (B) having a particle size of less than 3 ⁇ m obtained from the flow particle image analysis.
  • Ne(A) No(A) ⁇ F(A) (2)
  • Ne(B) No(B) ⁇ F(B) (3)
  • Carbon material (A) examples include artificial graphite, natural graphite, composite carbon material containing graphite and amorphous carbon, and the like. These carbon materials (A) may be used singly or in combination of two or more. Among these carbon materials (A), from the viewpoint of battery durability, artificial graphite, a composite carbon material containing graphite and amorphous carbon, and a mixture of a composite carbon material containing graphite and amorphous carbon and natural graphite are used. A composite carbon material containing graphite and amorphous carbon is preferred, and a mixture of a composite carbon material containing graphite and amorphous carbon and natural graphite is more preferred.
  • the mass ratio of graphite to amorphous carbon is 1 from the viewpoint of suppressing the specific surface area. : 0.01 or more is preferable, and 1:0.04 or more is more preferable.
  • the mass ratio of graphite and amorphous carbon is , 1:0.15 or less, and more preferably 1:0.10 or less.
  • the number of particles Ne(A) of the carbon material (A) is preferably 10 or more, more preferably 50 or more, from the viewpoint of ensuring electrical contact between particles and improving energy density.
  • the number of particles Ne(A) of the carbon material (A) is preferably 1000 or less, more preferably 900 or less, from the viewpoint of battery durability deterioration due to an increase in specific surface area.
  • the specific surface area of the carbon material (A) is preferably 0.5 m 2 /g or more, more preferably 1.0 m 2 /g or more.
  • the specific surface area of the carbon material (A) is preferably 5.0 m 2 /g or less, more preferably 3.0 m 2 /g or less, from the viewpoint of battery durability.
  • the average particle size of the carbon material (A) is preferably 5.0 ⁇ m or more, more preferably 8.0 ⁇ m or more.
  • the average particle size of the carbon material (A) is preferably 25.0 ⁇ m or less, more preferably 20.0 ⁇ m or less, from the viewpoint of ensuring electrical contact between particles.
  • the tap density of the carbon material (A) is preferably 1.00 g/cm 3 or more, more preferably 1.10 g/cm 3 or more, from the viewpoint of improving the energy density of the battery.
  • the tap density of the carbon material (A) is preferably 1.40 g/cm 3 or less, more preferably 1.30 g/cm 3 or less, from the viewpoint of ensuring electrical contact between particles.
  • Carbon material (B) examples include artificial graphite, natural graphite, composite carbon material containing graphite and amorphous carbon, and the like. These carbon materials (B) may be used singly or in combination of two or more. Among these carbon materials (B), artificial graphite, natural graphite, a mixture of artificial graphite and natural graphite, and graphite and amorphous carbon are used from the viewpoint of ensuring electrical contact between particles and battery durability. A composite carbon material containing carbon is preferable, and artificial graphite and natural graphite are more preferable.
  • the number of particles Ne(B) of the carbon material (B) is preferably 3,000 or more, more preferably 10,000 or more, from the viewpoint of ensuring electrical contact between particles.
  • the number of particles Ne(B) of the carbon material (B) is preferably 300,000 or less, more preferably 200,000 or less, from the viewpoint of battery durability deterioration due to an increase in specific surface area.
  • the specific surface area of the carbon material (B) is preferably 1.0 m 2 /g or more, more preferably 3.0 m 2 /g or more.
  • the specific surface area of the carbon material (A) is preferably 20.0 m 2 /g or less, more preferably 15.0 m 2 /g or less, from the viewpoint of battery durability.
  • the average particle size of the carbon material (B) is preferably 3 ⁇ m or more, more preferably 5 ⁇ m or more.
  • the average particle diameter of the carbon material (B) is preferably 15 ⁇ m or less, more preferably 10 ⁇ m or less, from the viewpoint of ensuring electrical contact between particles.
  • the tap density of the carbon material (B) is preferably 0.20 g/cm 3 or more, more preferably 0.30 g/cm 3 or more, from the viewpoint of improving the energy density of the battery.
  • the tap density of the carbon material (B) is preferably 1.20 g/cm 3 or less, more preferably 0.80 g/cm 3 or less, from the viewpoint of ensuring electrical contact between particles. It is more preferably 0.50 g/cm 3 or less.
  • pulverizers such as roller mills
  • impact pulverizers such as high-speed rotary pulverizers
  • air current impact pulverizers such as jet mills
  • dry swirling flow pulverizers A grinder or the like may be used.
  • composition of carbon material The composition of the carbon material when the carbon material (A) and the carbon material (B) are mixed to produce the carbon material of the present invention will be described.
  • the content C (A) of the carbon material (A) can maximize the electrical contact between particles within a range that does not impair the durability of the battery, so it is 70% by mass in the total 100% by mass of the carbon material. % or more, and more preferably 85 mass % or more.
  • the content C (A) of the carbon material (A) can ensure the minimum electrical contact between particles while maintaining the durability of the battery to the maximum. , is preferably 99% by mass or less, more preferably 98% by mass or less.
  • the content C (B) of the carbon material (B) can ensure the minimum electrical contact between the particles while maintaining the durability of the battery to the maximum. It is preferably at least 2% by mass, more preferably at least 2% by mass. On the other hand, the content C (B) of the carbon material (B) can maximize the electrical contact between particles within a range that does not impair the durability of the battery. It is preferably 30% by mass or less, more preferably 15% by mass or less.
  • the number of particles Nem (A) of the carbon material (A) in the entire carbon material is preferably 7 or more, and preferably 35 or more, from the viewpoint of ensuring electrical contact between particles and improving energy density. is more preferred.
  • the number of particles Nem (A) of the carbon material (A) in the entire carbon material is preferably 990 or less, more preferably 890 or less, from the viewpoint of battery durability deterioration due to an increase in specific surface area. more preferred.
  • the number of particles Nem(B) of the carbon material (B) in the entire carbon material is preferably 200 or more, more preferably 1000 or more, from the viewpoint of battery durability deterioration due to an increase in specific surface area. .
  • the number of particles Nem (B) of the carbon material (B) in the entire carbon material is preferably 30,000 or less, and preferably 20,000 or less, from the viewpoint of ensuring electrical contact between particles and improving energy density. It is more preferable to have
  • a rotating vessel type mixer typified by a horizontal cylinder type or a double cone type
  • a fixed vessel type mixer typified by a screw type or a ribbon type. They may be mixed using a fluid dynamic mixer typified by a jet pump type.
  • a secondary battery of the present invention includes a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode includes a current collector and a negative electrode active material layer formed on the current collector.
  • the carbon material of the present invention is contained in the active material layer, and the second embodiment of the present invention generally includes a step of forming a negative electrode active material layer using the carbon material of the present invention on a current collector to obtain a negative electrode. It is manufactured by the manufacturing method of the following battery.
  • a negative electrode using the carbon material of the present invention (hereinafter sometimes referred to as the “negative electrode of the present invention”), the carbon material of the present invention mixed with a binder (binder resin) is used as a dispersion medium. to form a slurry, which is applied to a current collector and dried to form a negative electrode active material layer on the current collector.
  • a binder binder resin
  • the binder use one that has an olefinic unsaturated bond in the molecule.
  • the type thereof is not particularly limited, specific examples include styrene-butadiene rubber, styrene/isoprene/styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, and ethylene/propylene/diene copolymer.
  • styrene-butadiene rubber is preferable because of its easy availability.
  • the binder having olefinic unsaturated bonds in the molecule it is desirable to have a large molecular weight or a high proportion of unsaturated bonds.
  • the weight average molecular weight is usually 10,000 or more, preferably 50,000 or more, and usually 1,000,000 or less, preferably 300,000 or less.
  • the number of moles of olefinic unsaturated bonds per 1 g of the total binder is usually 2.5 ⁇ 10 -7 or more, preferably 8 ⁇ 10 -7 or more, and usually A range of 5 ⁇ 10 ⁇ 6 or less, preferably 1 ⁇ 10 ⁇ 6 or less is desirable.
  • the binder should satisfy at least one of the regulations regarding the molecular weight and the regulations regarding the ratio of unsaturated bonds, but it is more preferable to satisfy both regulations at the same time. If the molecular weight of the binder having olefinically unsaturated bonds is too small, the mechanical strength will be poor, and if it is too large, the flexibility will be poor. If the proportion of olefinic unsaturated bonds in the binder is too low, the effect of improving the strength will be weak, and if it is too high, the flexibility will be poor.
  • the binder having olefinic unsaturated bonds has a degree of unsaturation of usually 15% or more, preferably 20% or more, more preferably 40% or more, and usually 90% or less, preferably 80% or less. is desirable.
  • the degree of unsaturation represents the ratio (%) of double bonds to the repeating units of the polymer.
  • binders having no olefinic unsaturated bonds can also be used in combination with binders having the above-mentioned olefinic unsaturated bonds as long as the effects of the present invention are not lost.
  • the mixing ratio of the binder having no olefinic unsaturated bonds to the amount of the binder having olefinic unsaturated bonds is usually 150% by mass or less, preferably 120% by mass or less.
  • binders having no olefinic unsaturated bonds include polysaccharides such as methylcellulose, carboxymethylcellulose and starch; thickening polysaccharides such as carrageenan, pullulan, guar gum and xanthan gum; polyethylene oxide, polypropylene oxide and the like.
  • the mass ratio of the carbon material of the present invention in the slurry and the binder (which may be a mixture of a binder having an unsaturated bond and a binder having no unsaturated bond as described above) (the Carbon material/binder) is usually 90/10 or more, preferably 95/5 or more, and usually 99.9/0.1 or less, preferably 99.5/0.5 or less in terms of dry mass ratio. Range. If the proportion of the binder is too high, the capacity tends to decrease and the resistance increases.
  • An organic solvent such as alcohol or water can be used as a dispersion medium for forming a slurry in which the carbon material and the binder of the present invention are dispersed.
  • a conductive agent may be added to the slurry.
  • the conductive agent include carbon black such as acetylene black, ketjen black, and furnace black, and fine powders of Cu, Ni, or alloys thereof having an average particle size of 1 ⁇ m or less.
  • the amount of the conductive agent added is usually about 10% by mass or less with respect to the carbon material of the present invention.
  • a conventionally known current collector can be used as the current collector to which the slurry is applied.
  • Specific examples include metal thin films such as rolled copper foil, electrolytic copper foil, and stainless steel foil.
  • the thickness of the current collector is usually 4 ⁇ m or more, preferably 6 ⁇ m or more, and usually 30 ⁇ m or less, preferably 20 ⁇ m or less.
  • the above slurry is applied onto a current collector using a doctor blade or the like, dried, and then pressed using a roll press or the like to form a negative electrode active material layer.
  • the slurry is preferably applied so that the amount of the carbon material of the present invention deposited on the current collector is 5 to 15 mg/cm 2 .
  • the drying after coating the slurry on the current collector is usually carried out at a temperature of 60°C or higher, preferably 80°C or higher, and usually 200°C or lower, preferably 195°C or lower, in dry air or an inert atmosphere.
  • the thickness of the negative electrode active material layer obtained by coating and drying the slurry is usually 5 ⁇ m or more, preferably 20 ⁇ m or more, more preferably 30 ⁇ m or more, usually 200 ⁇ m or less, preferably 100 ⁇ m or less, and more preferably 100 ⁇ m or less, in the state after pressing. is 75 ⁇ m or less. If the negative electrode active material layer is too thin, it lacks practicality as a negative electrode active material layer due to the balance with the particle size of the carbon material of the present invention, which is the negative electrode active material. If the negative electrode active material layer is too thick, it is difficult to obtain a sufficient Li ion intercalation/deintercalation function for a high-density current value.
  • the density of the carbon material of the present invention in the negative electrode active material layer varies depending on the application, but is preferably 1.5 g/cm 3 or more, more preferably 1.54 g/cm 3 or more. 6 g/cm 3 or more, more preferably 1.65 g/cm 3 or more, particularly 1.7 g/cm 3 or more. If the density is too low, the battery capacity per unit volume is not necessarily sufficient. On the other hand, if the density is too high, the rate characteristics deteriorate, so the density of the carbon material of the present invention is preferably 1.9 g/cm 3 or less.
  • the method and selection of other materials are not particularly limited. Also, when a secondary battery is produced using this negative electrode, there is no particular restriction on the selection of members necessary for the battery configuration, such as the positive electrode and the electrolytic solution that constitute the secondary battery.
  • a secondary battery of the present invention generally comprises a positive electrode and a negative electrode capable of intercalating and deintercalating lithium ions, and an electrolyte.
  • the negative electrode the negative electrode of the present invention described above is used.
  • the positive electrode is formed by forming a positive electrode active material layer containing a positive electrode active material and a binder on a current collector.
  • positive electrode active materials include metal chalcogen compounds capable of intercalating and deintercalating alkali metal cations such as lithium ions during charging and discharging.
  • Metal chalcogen compounds include transition metal oxides such as vanadium oxide, molybdenum oxide, manganese oxide, chromium oxide, titanium oxide, tungsten oxide; vanadium sulfide, molybdenum sulfide transition metal sulfides such as sulfides, titanium sulfides, and CuS; transition metal phosphorus-sulfur compounds such as NiPS 3 and FePS 3 ; transition metal selenium compounds such as VSe 2 and NbSe 3 ; transition metal composite oxides such as 75 S 2 and Na 0.1 CrS 2 ; transition metal composite sulfides such as LiCoS 2 and LiNiS 2 ;
  • V2O5 , V5O13 , VO2 , Cr2O5 , MnO2 , TiO , MoV2O8 , LiCoO2 , LiNiO2 , LiMn2O4 , TiS2 , V2S5 , Cr 0.25 V 0.75 S 2 , Cr 0.5 V 0.5 S 2 and the like are preferable, and LiCoO 2 , LiNiO 2 , LiMn 2 O 4 and a part of these transition metals are particularly preferable. It is a lithium transition metal composite oxide substituted with other metals.
  • These positive electrode active materials may be used singly or in combination.
  • any known binder can be selected and used.
  • examples thereof include inorganic compounds such as silicate and water glass, and resins having no unsaturated bonds such as Teflon (registered trademark) and polyvinylidene fluoride. Among these, resins having no unsaturated bonds are preferred. If a resin having an unsaturated bond is used as the resin that binds the positive electrode active material, it may decompose during an oxidation reaction (during charging).
  • the weight average molecular weight of these resins is usually 10,000 or more, preferably 100,000 or more, and usually 3,000,000 or less, preferably 1,000,000 or less.
  • a conductive agent may be contained in the positive electrode active material layer in order to improve the conductivity of the electrode.
  • the conductive agent is not particularly limited as long as it can be mixed with the active material in an appropriate amount to impart conductivity.
  • Examples of conductive agents generally include carbon powders such as acetylene black, carbon black, and graphite, and fibers, powders, and foils of various metals.
  • the positive electrode plate is formed by slurrying the positive electrode active material and binder with a dispersant, applying it on the current collector, and drying it, in the same manner as in the manufacturing of the negative electrode of the present invention described above.
  • Aluminum, nickel, stainless steel (SUS), or the like is used as the current collector of the positive electrode, but is not limited at all.
  • a non-aqueous electrolytic solution obtained by dissolving a lithium salt in a non-aqueous solvent, or a non-aqueous electrolytic solution made into a gel, rubber, or solid sheet by using an organic polymer compound or the like is used.
  • the non-aqueous solvent used in the non-aqueous electrolyte is not particularly limited, and can be appropriately selected and used from known non-aqueous solvents that have been conventionally proposed as solvents for non-aqueous electrolytes.
  • chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate
  • cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate
  • chain ethers such as 1,2-dimethoxyethane
  • tetrahydrofuran, 2-methyl Cyclic ethers such as tetrahydrofuran, sulfolane and 1,3-dioxolane
  • chain esters such as methyl formate, methyl acetate and methyl propionate
  • cyclic esters such as ⁇ -butyrolactone and ⁇ -valerolactone.
  • any one of these non-aqueous solvents may be used alone, or two or more thereof may be used in combination.
  • a mixed solvent a combination of a mixed solvent containing a cyclic carbonate and a chain carbonate is preferable, and the cyclic carbonate is a mixed solvent of ethylene carbonate and propylene carbonate. It is particularly preferable in that load characteristics are improved.
  • the content of propylene carbonate is preferably in the range of 2% by mass to 80% by mass, more preferably 5% by mass to 70% by mass, and 10% by mass to 60% by mass with respect to the entire non-aqueous solvent. A range is more preferred. If the content of propylene carbonate is lower than the above lower limit, the ionic conductivity at low temperatures decreases. If the content of propylene carbonate is higher than the above upper limit, propylene carbonate solvated with Li ions co-inserts between the graphite phases of the negative electrode, causing delamination deterioration of the graphite-based negative electrode active material, and sufficient capacity cannot be obtained. There's a problem.
  • the lithium salt used in the non-aqueous electrolytic solution is also not particularly limited, and can be appropriately selected and used from known lithium salts known to be usable for this purpose.
  • Li halides such as Cl, LiBr; perhalogenates such as LiClO4 , LiBrO4 , LiClO4 ; inorganic lithium salts such as inorganic fluoride salts such as LiPF6 , LiBF4 , LiAsF6 ; LiCF3SO3 , LiC4 perfluoroalkanesulfonate such as F 9 SO 3 ; fluorine-containing organic lithium salt such as perfluoroalkanesulfonimide salt such as Li trifluorosulfonimide ((CF 3 SO 2 ) 2 NLi);
  • LiClO 4 , LiPF 6 and LiBF 4 are preferred.
  • the lithium salt may be used alone or in combination of two or more.
  • concentration of the lithium salt in the non-aqueous electrolytic solution is usually in the range of 0.5 mol/L or more and 2.0 mol/L or less.
  • organic polymer compound When an organic polymer compound is added to the above non-aqueous electrolytic solution and the electrolyte is used in the form of a gel, rubber, or solid sheet, specific examples of the organic polymer compound include polyethylene oxide, polypropylene oxide, and the like.
  • Polyether-based polymer compounds are crosslinked polymers of polyether-based polymer compounds; Vinyl alcohol-based polymer compounds such as polyvinyl alcohol and polyvinyl butyral; Insolubilized vinyl alcohol-based polymer compounds; Siloxane; vinyl polymer compounds such as polyvinylpyrrolidone, polyvinylidene carbonate, polyacrylonitrile; poly( ⁇ -methoxyoligooxyethylene methacrylate), poly( ⁇ -methoxyoligooxyethylene methacrylate-co-methyl methacrylate), poly(hexafluoro and polymer copolymers such as propylene-vinylidene fluoride).
  • the non-aqueous electrolytic solution described above may further contain a film-forming agent.
  • film-forming agents include carbonate compounds such as vinylene carbonate, vinyl ethyl carbonate and methylphenyl carbonate; alkene sulfides such as ethylene sulfide and propylene sulfide; sultone compounds such as 1,3-propanesultone and 1,4-butanesultone. and acid anhydrides such as maleic anhydride and succinic anhydride.
  • the non-aqueous electrolytic solution may contain an overcharge inhibitor such as diphenyl ether or cyclohexylbenzene.
  • the content in the non-aqueous electrolytic solution is usually 10% by mass or less, preferably 8% by mass or less, more preferably 5% by mass or less, and particularly preferably 2% by mass or less. If the content of the additive is too large, other battery characteristics may be adversely affected, such as an increase in initial irreversible capacity, deterioration in low-temperature characteristics and rate characteristics.
  • a polymer solid electrolyte which is a conductor of alkali metal cations such as lithium ions
  • examples of polymer solid electrolytes include those obtained by dissolving Li salts in the aforementioned polyether-based polymer compounds, and polymers in which terminal hydroxyl groups of polyethers are substituted with alkoxides.
  • a porous separator such as a porous membrane or non-woven fabric is usually interposed between the positive electrode and the negative electrode to prevent a short circuit between the electrodes.
  • the non-aqueous electrolytic solution is used by impregnating a porous separator.
  • polyolefins such as polyethylene and polypropylene, polyethersulfone, and the like are used, and polyolefins are preferred.
  • the form of the lithium ion secondary battery to which the present invention is applied is not particularly limited. Examples include a cylinder type in which a sheet electrode and a separator are formed in a spiral shape, a cylinder type in which a pellet electrode and a separator are combined to form an inside-out structure, and a coin type in which a pellet electrode and a separator are laminated.
  • a cylinder type in which a sheet electrode and a separator are formed in a spiral shape
  • a cylinder type in which a pellet electrode and a separator are combined to form an inside-out structure
  • a coin type in which a pellet electrode and a separator are laminated.
  • a negative electrode is placed on an exterior case, an electrolytic solution and a separator are provided thereon, a positive electrode is placed so as to face the negative electrode, and a gasket and a sealing plate are crimped together to form a battery.
  • the secondary battery of the present invention uses the carbon material of the present invention as a negative electrode active material, and thus has excellent cycle characteristics.
  • the capacity retention rate after 500 cycles measured by the method described in Examples below is preferably 91.0% or more, particularly 92.0% or more.
  • the DCR retention rate after 500 cycles measured by the method described in Examples below is preferably 160% or less, particularly 150% or less.
  • Ne/Ne (A)/Ne (B)> The carbon materials obtained in Examples and Comparative Examples, and the carbon materials (A) and (B) used in Examples and Comparative Examples were analyzed by a flow-type particle image analyzer (model name "FPIA", Sysmex Corporation ) was used to measure the number of particles. Specifically, about 0.2 g of the sample is dispersed in a 0.2% by mass aqueous solution (about 50 mL) of polyoxyethylene (20) sorbitan monolaurate, which is a surfactant, and ultrasonic waves are applied at 28 kHz at an output of 60 W.
  • a flow-type particle image analyzer model name "FPIA", Sysmex Corporation
  • the detection range is specified as 0.6 to 40 ⁇ m, and the number of particles (No, No (A), No (B)) of the carbon material, carbon material (A), and carbon material (B),
  • the appearance frequency (F F (A) F (B)) of particles of carbon material, carbon material (A), and carbon material (B) having a particle size of less than 3 ⁇ m is measured, and the following formulas (1) to (3 ).
  • Ne No ⁇ F (1)
  • Ne(A) No(A) ⁇ F(A) (2)
  • Ne(B) No(B) ⁇ F(B) (3)
  • Nem (A) and Nem (B) ⁇ Number of particles Nem (A) and Nem (B)> Regarding the carbon material (A) and the carbon material (B) used in the examples and comparative examples, the number of particles (Ne (A) Ne (B)) calculated above and the content rate (C (A) C ( B)) and calculated by the following formulas (4) to (5)
  • Nem (A) Ne (A) ⁇ C (A) ⁇ 100 (%)
  • Nem (B) Ne (B) x C (B) ⁇ 100 (%) (5)
  • the number of peaks was measured from the particle size distribution measured by flow particle image analysis. Specifically, about 0.2 g of the sample is dispersed in a 0.2% by mass aqueous solution (about 50 mL) of polyoxyethylene (20) sorbitan monolaurate, which is a surfactant, and ultrasonic waves are applied at 28 kHz at an output of 60 W. After irradiation for 1 minute, the particle size distribution of the carbon material, carbon material (A), and carbon material (B) was obtained by setting the detection range to 0.6 to 40 ⁇ m. The number of peaks was measured from the obtained particle size distribution. Also, for the carbon material, the grain size at which a peak exists was determined.
  • ⁇ Average particle size> For the carbon materials obtained in Examples and Comparative Examples, and the carbon materials (A) and (B) used in Examples and Comparative Examples, from the volume-based particle size distribution measured by laser diffraction, the average particle size Diameter was measured. Specifically, about 2.0 g of the sample was added to about 150 mL of a 0.1 vol% aqueous solution of polyoxyethylene (20) sorbitan monolaurate (Tween 20 (registered trademark)), which is a surfactant, and 0.01 g of the sample was added.
  • polyoxyethylene (20) sorbitan monolaurate Teween 20 (registered trademark)
  • LA-920 manufactured by HORIBA
  • HORIBA laser diffraction/scattering particle size distribution analyzer
  • a specific surface area measuring device model name "AMS8000", manufactured by Okura Riken Co., Ltd.
  • the specific surface area was measured by the BET one-point method by the nitrogen gas adsorption flow method. Specifically, 0.4 g of the sample is filled in the cell, heated to 350° C. for pretreatment, cooled to the temperature of liquid nitrogen, and 30% nitrogen and 70% helium gas is saturated and adsorbed, Then, the amount of desorbed gas was measured by heating to room temperature, and the specific surface area was calculated by the BET method from the obtained results.
  • ⁇ Tap density> For the carbon materials obtained in Examples and Comparative Examples, and the carbon materials (A) and (B) used in Examples and Comparative Examples, a powder density measuring instrument (model name "Tap Denser KYT-4000" (manufactured by Seishin Enterprise Co., Ltd.), a cylindrical tap cell with a diameter of 1.6 cm and a volume capacity of 20 cm 3 is passed through a sieve with an opening of 300 ⁇ m, and the sample is dropped to fill the cell to the full. Tapping was performed 1000 times, and the density calculated from the volume at that time and the mass of the sample was taken as the tap density.
  • Sphericalized graphite (average particle diameter: 16.0 ⁇ m, BET specific surface area: 6.9 m 2 /g, tap density: 1.06 g/cm 3 ) was obtained by spheroidizing flake natural graphite with an average particle diameter of 100 ⁇ m. This spheroidized graphite was packed in a rubber container, sealed, isotropically pressurized at 200 MPa, and then pulverized and classified to obtain a spheroidized graphite powder.
  • the pressure in the furnace was increased to 10 torr. Then, the pressure was reduced to atmospheric pressure with nitrogen, and the oxygen concentration in the furnace was reduced to less than 100 ppm by circulating nitrogen, followed by heat treatment at 1300°C.
  • the obtained fired product was pulverized and classified to obtain a carbon material (A-1) containing an amorphous carbonaceous material on the surface of spherical graphite.
  • the obtained carbon material (A-1) had a mass ratio of spheroidized graphite to amorphous carbon (spheroidized graphite:amorphous carbon) of 1:0.05.
  • Sphericalized graphite (average particle diameter: 16.0 ⁇ m, BET specific surface area: 6.9 m 2 /g, tap density: 1.06 g/cm 3 ) was obtained by spheroidizing flake natural graphite with an average particle diameter of 100 ⁇ m. After mixing this spheroidized graphite with pitch adjusted to have an ash content of 0.02% by mass, a metal impurity amount of 20% by mass, and a Qi of 1% by mass as an amorphous carbon precursor, the pressure in the furnace was reduced to 10 torr or less.
  • the obtained fired product was pulverized and classified to obtain a carbon material (A-2) containing an amorphous carbonaceous material on the surface of spherical graphite.
  • the obtained carbon material (A-2) had a mass ratio of spheroidized graphite to amorphous carbon (spheroidized graphite:amorphous carbon) of 1:0.055.
  • Sphericalized graphite (average particle diameter: 16.0 ⁇ m, BET specific surface area: 6.9 m 2 /g, tap density: 1.06 g/cm 3 ) was obtained by spheroidizing flake natural graphite with an average particle diameter of 100 ⁇ m. This spheroidized graphite was packed in a rubber container, sealed, isotropically pressurized at 200 MPa, and then pulverized and classified to obtain a spheroidized graphite powder.
  • the pressure in the furnace is reduced to 10 torr or less. Then, the pressure was restored to the atmospheric pressure with nitrogen, and the oxygen concentration in the furnace was reduced to less than 100 ppm by circulating nitrogen, and heat treatment was performed at 1300°C.
  • the obtained fired product was pulverized and classified to obtain a carbon material (A-3) containing an amorphous carbonaceous material on the surface of spherical graphite.
  • the obtained carbon material (A-3) had a mass ratio of spheroidized graphite to amorphous carbon (spheroidized graphite:amorphous carbon) of 1:0.03.
  • Sphericalized graphite (average particle size: 9.6 ⁇ m, BET specific surface area: 8.3 m 2 /g, tap density: 0.69 g/cm 3 ) was obtained by spheroidizing flake natural graphite with an average particle size of 100 ⁇ m. After mixing this spheroidized graphite with pitch adjusted to have an ash content of 0.02% by mass, a metal impurity amount of 20% by mass, and a Qi of 1% by mass as an amorphous carbon precursor, the pressure in the furnace was reduced to 10 torr or less.
  • the obtained fired product was pulverized and classified to obtain a carbon material (A-4) containing an amorphous carbonaceous material on the surface of spherical graphite.
  • the obtained carbon material (A-4) had a mass ratio of spheroidized graphite to amorphous carbon (spheroidized graphite:amorphous carbon) of 1:0.075.
  • a carbon material (B-1) was obtained by spheroidizing flake natural graphite having an average particle size of 100 ⁇ m.
  • a carbon material (B'-1) was obtained by spheroidizing flake natural graphite having an average particle size of 100 ⁇ m.
  • the resulting slurry was applied to one side of a rolled copper foil having a thickness of 10 ⁇ m, dried, and rolled with a press to obtain a negative electrode active material layer with a width of 30 mm and a length of 40 mm, and a current collector tab weld. A shape having an uncoated portion was cut out to obtain a negative electrode. At this time, the thickness of the negative electrode active material layer was about 60 ⁇ m, and the density of the carbon material was 1.60 to 1.70 g/cm 3 .
  • the positive electrode active material is a lithium-transition metal composite oxide synthesized by the method described below and represented by the composition formula LiMn 0.33 Ni 0.33 Co 0.33 O 2 .
  • a slurry was prepared, and while stirring, the solid content in the slurry was wet pulverized using a circulating medium stirring wet bead mill so that the volume-based average particle diameter d50 was 0.2 ⁇ m.
  • the obtained slurry was spray-dried with a spray dryer to obtain almost spherical granulated particles having a particle diameter of about 5 ⁇ m and consisting only of the manganese raw material, the nickel raw material and the cobalt raw material.
  • LiOH powder having a volume-based average particle diameter d50 of 3 ⁇ m was added to the obtained granulated particles so that the ratio of the number of moles of Li to the total number of moles of Mn, Ni, and Co was 1.05.
  • Mixing was performed by a speed mixer to obtain a mixed powder of granulated particles of the nickel raw material, the cobalt raw material and the manganese raw material and the lithium raw material. This mixed powder was sintered at 950° C.
  • This positive electrode active material had a BET specific surface area of 1 m 2 /g, an average primary particle size of 1 ⁇ m, a volume-based average particle size d50 of 8 ⁇ m, and a tap density of 1.7 g/cm 3 .
  • a current collecting tab is welded to the uncoated portion of each of the positive electrode and the negative electrode, and the electrode body is a laminate sheet in which a polypropylene film, a 0.04 mm thick aluminum foil, and a nylon film are laminated in this order (total thickness 0.1 mm), sandwiched between laminate sheets with the polypropylene film on the inner side, and except for one piece for injecting the electrolytic solution, the region without the electrode was heat-sealed. After that, 235 ⁇ L of the non-aqueous electrolyte was injected into the active material layer to sufficiently permeate the electrode and sealed to produce a laminate cell. The rated capacity of this battery is 33 mAh.
  • Capacity retention rate after 500 cycles (Discharge capacity at 500th cycle / Discharge capacity at 1st cycle) x 100
  • DCR maintenance rate after 500 cycles (DCR after 500 cycles/Initial DCR) x 100 10 at current values 0.2C, 0.5C, 1.0C, 2.0C, and 3.0C for batteries adjusted in advance to SOC 50% (state of charge) in an environment of -30°C. After discharging for 10 seconds, the amount of voltage drop is measured. DCR ( ⁇ ) is calculated from the slope of the voltage drop amount (V)-current value (A) curve thus obtained.
  • Table 2 shows the evaluation results of the battery performance of the carbon materials prepared in each example and comparative example, together with the specific surface area, volume average particle diameter (d50), tap density and peak position.
  • the carbon material of the present invention having a particle size distribution with a peak number of 2 or more, a particle number Ne of 700 or more, and a specific surface area of 10 m 2 /g or less can be used as a negative electrode active material. , it is possible to provide a secondary battery having excellent cycle characteristics, capacity retention rate after 500 cycles, and DCR retention rate after 500 cycles.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Electrochemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Inorganic Chemistry (AREA)
  • Organic Chemistry (AREA)
  • Manufacturing & Machinery (AREA)
  • Materials Engineering (AREA)
  • Geology (AREA)
  • General Life Sciences & Earth Sciences (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Battery Electrode And Active Subsutance (AREA)
PCT/JP2022/037832 2021-10-28 2022-10-11 炭素材及びその製造方法と、二次電池及びその製造方法 Ceased WO2023074346A1 (ja)

Priority Applications (6)

Application Number Priority Date Filing Date Title
CN202280071387.2A CN118159490A (zh) 2021-10-28 2022-10-11 碳材料及其制造方法、二次电池及其制造方法
KR1020247009172A KR20240087705A (ko) 2021-10-28 2022-10-11 탄소재 및 그 제조 방법과, 이차 전지 및 그 제조 방법
JP2023556283A JPWO2023074346A1 (cg-RX-API-DMAC7.html) 2021-10-28 2022-10-11
CA3233421A CA3233421A1 (en) 2021-10-28 2022-10-11 Carbon material and production method therefor, and secondary battery and manufacturing method therefor
EP22886676.0A EP4424636A4 (en) 2021-10-28 2022-10-11 CARBON MATERIAL AND ITS PRODUCTION METHOD, AND SECONDARY BATTERY AND ITS MANUFACTURING METHOD
US18/621,202 US20240243286A1 (en) 2021-10-28 2024-03-29 Carbon material and production method therefor, and secondary battery and manufacturing method therefor

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021-176633 2021-10-28
JP2021176633 2021-10-28

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US18/621,202 Continuation US20240243286A1 (en) 2021-10-28 2024-03-29 Carbon material and production method therefor, and secondary battery and manufacturing method therefor

Publications (1)

Publication Number Publication Date
WO2023074346A1 true WO2023074346A1 (ja) 2023-05-04

Family

ID=86157882

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/037832 Ceased WO2023074346A1 (ja) 2021-10-28 2022-10-11 炭素材及びその製造方法と、二次電池及びその製造方法

Country Status (8)

Country Link
US (1) US20240243286A1 (cg-RX-API-DMAC7.html)
EP (1) EP4424636A4 (cg-RX-API-DMAC7.html)
JP (1) JPWO2023074346A1 (cg-RX-API-DMAC7.html)
KR (1) KR20240087705A (cg-RX-API-DMAC7.html)
CN (1) CN118159490A (cg-RX-API-DMAC7.html)
CA (1) CA3233421A1 (cg-RX-API-DMAC7.html)
TW (1) TW202322438A (cg-RX-API-DMAC7.html)
WO (1) WO2023074346A1 (cg-RX-API-DMAC7.html)

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013201104A (ja) 2011-03-29 2013-10-03 Mitsubishi Chemicals Corp 非水系二次電池用負極炭素材、及び負極並びに、非水系二次電池
JP2016091632A (ja) * 2014-10-30 2016-05-23 日立マクセル株式会社 リチウムイオン二次電池
WO2017057123A1 (ja) * 2015-09-30 2017-04-06 Necエナジーデバイス株式会社 リチウムイオン二次電池用負極及びリチウムイオン二次電池
JP2021176633A (ja) 2015-06-18 2021-11-11 ジョンソン、マッセイ、パブリック、リミテッド、カンパニーJohnson Matthey Public Limited Company 低n2o形成性を有するアンモニアスリップ触媒

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP6040022B2 (ja) * 2012-03-02 2016-12-07 Jfeケミカル株式会社 リチウムイオン二次電池用負極材料、リチウムイオン二次電池用負極およびリチウムイオン二次電池
US12476251B2 (en) * 2019-10-04 2025-11-18 Lg Energy Solution, Ltd. Globular carbon-based anode active material, method for manufacturing same, and anode and lithium secondary battery comprising same
CN112436104B (zh) * 2020-12-30 2022-09-06 兰溪致德新能源材料有限公司 负极极片及其制备方法

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013201104A (ja) 2011-03-29 2013-10-03 Mitsubishi Chemicals Corp 非水系二次電池用負極炭素材、及び負極並びに、非水系二次電池
JP2016091632A (ja) * 2014-10-30 2016-05-23 日立マクセル株式会社 リチウムイオン二次電池
JP2021176633A (ja) 2015-06-18 2021-11-11 ジョンソン、マッセイ、パブリック、リミテッド、カンパニーJohnson Matthey Public Limited Company 低n2o形成性を有するアンモニアスリップ触媒
WO2017057123A1 (ja) * 2015-09-30 2017-04-06 Necエナジーデバイス株式会社 リチウムイオン二次電池用負極及びリチウムイオン二次電池

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4424636A4

Also Published As

Publication number Publication date
JPWO2023074346A1 (cg-RX-API-DMAC7.html) 2023-05-04
US20240243286A1 (en) 2024-07-18
KR20240087705A (ko) 2024-06-19
CA3233421A1 (en) 2023-05-04
EP4424636A4 (en) 2025-07-16
CN118159490A (zh) 2024-06-07
EP4424636A1 (en) 2024-09-04
TW202322438A (zh) 2023-06-01

Similar Documents

Publication Publication Date Title
CN1127774C (zh) 非水电解质二次电池
KR102705366B1 (ko) 음극 및 이를 포함하는 이차전지
CN114464774B (zh) 一种负极极片及其应用
JP5582587B2 (ja) リチウムイオン二次電池
WO2016136178A1 (ja) 非水電解質二次電池用負極及び非水電解質二次電池
JPWO2011115247A1 (ja) リチウムイオン二次電池
JP7548197B2 (ja) リチウム複合酸化物、蓄電デバイス及びリチウム複合酸化物の製造方法
JP7731342B2 (ja) 非水電解質二次電池
JP2013229301A (ja) 負極及びリチウムイオン二次電池
JP2005294079A (ja) 二次電池用負極、その製造方法及び二次電池
JP4513385B2 (ja) 二次電池用負極及び二次電池
JP2013134921A (ja) 非水電解質二次電池用電極および非水電解質二次電池
JP2025518058A (ja) 二次電池及びその製造方法と電力消費装置
JP5017010B2 (ja) リチウム二次電池
WO2014115322A1 (ja) リチウムイオン二次電池用負極活物質及びそれらを用いたリチウムイオン二次電池
JP4867153B2 (ja) 非水電解液二次電池用の正極活物質、二次電池用正極および非水電解液二次電池
JP2010176973A (ja) 非水電解質二次電池
US20240243286A1 (en) Carbon material and production method therefor, and secondary battery and manufacturing method therefor
JP7798634B2 (ja) 電極、蓄電デバイス及び電極の製造方法
JP7529704B2 (ja) 正極およびこれを備える二次電池
JP2025154208A (ja) リチウムイオン二次電池およびリチウムイオン二次電池モジュール
JP2025154204A (ja) リチウムイオン二次電池およびリチウムイオン二次電池モジュール
JP2025154209A (ja) リチウムイオン二次電池およびリチウムイオン二次電池モジュール
JP2025154206A (ja) リチウムイオン二次電池およびリチウムイオン二次電池モジュール
JP2025059130A (ja) 蓄電デバイス

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22886676

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2023556283

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 3233421

Country of ref document: CA

WWE Wipo information: entry into national phase

Ref document number: 202280071387.2

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 202447033258

Country of ref document: IN

WWE Wipo information: entry into national phase

Ref document number: 2022886676

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2022886676

Country of ref document: EP

Effective date: 20240528