WO2022270358A1 - 感光性着色樹脂組成物、硬化物、カラーフィルタ、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 - Google Patents
感光性着色樹脂組成物、硬化物、カラーフィルタ、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 Download PDFInfo
- Publication number
- WO2022270358A1 WO2022270358A1 PCT/JP2022/023797 JP2022023797W WO2022270358A1 WO 2022270358 A1 WO2022270358 A1 WO 2022270358A1 JP 2022023797 W JP2022023797 W JP 2022023797W WO 2022270358 A1 WO2022270358 A1 WO 2022270358A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- group
- mass
- carbon atoms
- resin composition
- photosensitive colored
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/09—Photosensitive materials characterised by structural details, e.g. supports, auxiliary layers
- G03F7/105—Photosensitive materials characterised by structural details, e.g. supports, auxiliary layers having substances, e.g. indicators, for forming visible images
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B5/00—Optical elements other than lenses
- G02B5/20—Filters
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/027—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/027—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds
- G03F7/028—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds with photosensitivity-increasing substances, e.g. photoinitiators
- G03F7/031—Organic compounds not covered by group G03F7/029
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/027—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds
- G03F7/032—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds with binders
- G03F7/033—Non-macromolecular photopolymerisable compounds having carbon-to-carbon double bonds, e.g. ethylenic compounds with binders the binders being polymers obtained by reactions only involving carbon-to-carbon unsaturated bonds, e.g. vinyl polymers
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/038—Macromolecular compounds which are rendered insoluble or differentially wettable
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03F—PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR
- G03F7/00—Photomechanical, e.g. photolithographic, production of textured or patterned surfaces, e.g. printing surfaces; Materials therefor, e.g. comprising photoresists; Apparatus specially adapted therefor
- G03F7/004—Photosensitive materials
- G03F7/039—Macromolecular compounds which are photodegradable, e.g. positive electron resists
-
- G—PHYSICS
- G09—EDUCATION; CRYPTOGRAPHY; DISPLAY; ADVERTISING; SEALS
- G09F—DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS
- G09F9/00—Indicating arrangements for variable information in which the information is built-up on a support by selection or combination of individual elements
- G09F9/30—Indicating arrangements for variable information in which the information is built-up on a support by selection or combination of individual elements in which the desired character or characters are formed by combining individual elements
-
- H—ELECTRICITY
- H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
- H05B—ELECTRIC HEATING; ELECTRIC LIGHT SOURCES NOT OTHERWISE PROVIDED FOR; CIRCUIT ARRANGEMENTS FOR ELECTRIC LIGHT SOURCES, IN GENERAL
- H05B33/00—Electroluminescent light sources
- H05B33/02—Details
-
- H—ELECTRICITY
- H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
- H05B—ELECTRIC HEATING; ELECTRIC LIGHT SOURCES NOT OTHERWISE PROVIDED FOR; CIRCUIT ARRANGEMENTS FOR ELECTRIC LIGHT SOURCES, IN GENERAL
- H05B33/00—Electroluminescent light sources
- H05B33/10—Apparatus or processes specially adapted to the manufacture of electroluminescent light sources
-
- H—ELECTRICITY
- H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
- H05B—ELECTRIC HEATING; ELECTRIC LIGHT SOURCES NOT OTHERWISE PROVIDED FOR; CIRCUIT ARRANGEMENTS FOR ELECTRIC LIGHT SOURCES, IN GENERAL
- H05B33/00—Electroluminescent light sources
- H05B33/12—Light sources with substantially two-dimensional [2D] radiating surfaces
Definitions
- the present invention relates to a photosensitive colored resin composition, a cured product, a color filter, a display device, and a method for producing a laminate of an organic light-emitting element and an external light antireflection film using the photosensitive colored resin composition.
- an organic light emitting element emitting white light or an inorganic light emitting element emitting white light may be used.
- An organic light-emitting display device uses a color filter for color adjustment.
- the color filter is generally formed on a substrate, a colored layer formed on the substrate and composed of colored patterns of the three primary colors of red, green, and blue, and formed on the substrate so as to partition each colored pattern. and a light shielding part.
- a method for forming a colored layer in a color filter for example, a colored resin composition obtained by adding a binder resin, a photopolymerizable compound and a photoinitiator to a coloring material dispersion liquid in which a coloring material is dispersed using a dispersing agent or the like is prepared. After being coated on a substrate and dried, it is exposed to light using a photomask and developed to form a colored pattern, which is fixed by heating to form a colored layer.
- a colored resin composition is applied to a substrate in a pattern by an inkjet method or the like, dried, and then cured to form a colored pattern, and the pattern is fixed by heating to form a colored layer. Formation These steps are repeated for each color to form a color filter.
- the cross-sectional shape of the resulting pattern tends to be an undercut shape (also called a reverse tapered shape), that is, a shape in which the top surface of the pattern is the widest and the bottom surface is the narrowest.
- Undercut shapes cause various problems, such as pattern peeling and chipping, gaps at the edges of pixels, and uneven coating when applied to the top in the next process. become
- Patent Document 1 a non-reactive alkali-soluble resin and a photopolymerization initiator (A ), the photopolymerization initiator (A) contains a photopolymerization initiator (a1) containing two oxime groups in one molecule, and the glass transition temperature (Tg) of the non-reactive alkali-soluble resin is , and a temperature of 0° C. or lower.
- the colored photosensitive resin composition of Patent Document 1 contains a resin having a low glass transition temperature, so that post-baking belonging to high heat treatment such as 220 ° C. in the color filter manufacturing process is performed to melt and flow the colored layer. It is a technique that enables formation of a forward tapered pattern after the baking process.
- the present invention has been made in view of the above circumstances, and provides a photosensitive colored resin composition capable of suppressing the generation of development residues even in low-temperature heat treatment and forming a colored layer with a good pattern shape. With the goal.
- the present invention also provides a color filter and a display device formed using the photosensitive colored resin composition, and a laminate of an organic light-emitting element and an external light antireflection film using the photosensitive colored resin composition.
- the object is to provide a manufacturing method.
- the photosensitive colored resin composition according to the present invention contains a coloring material, an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and a solvent,
- the alkali-soluble resin has an acid value of more than 50 mgKOH/g
- the non-reactive resin has an acid value of 7 mgKOH/g to 50 mgKOH/g, a content of structural units derived from methyl methacrylate in all structural units of 50% to 99% by mass, and a weight average molecular weight of 5000 to 50000.
- the cured product according to the present invention is the cured product of the photosensitive colored resin composition according to the present invention.
- the color filter according to the present invention is a color filter comprising at least a substrate and a colored layer provided on the substrate, wherein at least one of the colored layers is a cured photosensitive colored resin composition according to the present invention. It is a thing.
- a display device has the color filter according to the present invention. Further, the display device according to the present invention has a cured film of the photosensitive colored resin composition according to the present invention on the organic light-emitting element.
- a method for manufacturing a laminate of an organic light-emitting element and an external light antireflection film according to the present invention includes: A step of forming a coating film by applying the photosensitive colored resin composition according to the present invention on the organic light emitting device; a step of irradiating the coating film with light; A post-baking step of heating the film after the light irradiation, and By including the step of developing the film after the light irradiation, A step of forming a cured film of the photosensitive colored resin composition according to the present invention on the organic light-emitting element.
- a photosensitive colored resin composition capable of suppressing the generation of development residues and forming a colored layer with a good pattern shape even when subjected to low-temperature heat treatment.
- a color filter and a display device formed using the photosensitive colored resin composition, and a laminate of an organic light emitting device and an external light antireflection film using the photosensitive colored resin composition A method of manufacturing a body can be provided.
- FIG. 1 is a schematic cross-sectional view showing an example of a color filter according to the invention.
- FIG. 2 is a schematic cross-sectional view showing an example of a liquid crystal display device according to the present invention.
- FIG. 3 is a schematic cross-sectional view showing an example of an organic light-emitting display device according to the present invention.
- FIG. 4 is a schematic cross-sectional view showing another example of a display device having an organic light-emitting device according to the present invention.
- FIG. 5 is a schematic cross-sectional view for explaining the taper angle ( ⁇ 1) of the cross-sectional shape of the colored layer.
- light includes electromagnetic waves with wavelengths in the visible and non-visible regions, and radiation, and radiation includes, for example, microwaves and electron beams. Specifically, it refers to electromagnetic waves with a wavelength of 5 ⁇ m or less and electron beams.
- (meth)acryloyl represents acryloyl and methacryloyl
- (meth)acryl represents acrylic and methacrylic
- (meth)acrylate represents acrylate and methacrylate.
- the term "to" indicating a numerical range is used to include the numerical values before and after it as lower and upper limits.
- the photosensitive colored resin composition, the cured product, the color filter, the display device, and the method for producing the laminate of the organic light-emitting element and the external light antireflection film according to the present invention will be described in detail in order.
- the photosensitive colored resin composition according to the present invention contains a colorant, an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and a solvent,
- the alkali-soluble resin has an acid value of more than 50 mgKOH/g
- the non-reactive resin has an acid value of 7 mgKOH/g to 50 mgKOH/g, a content of structural units derived from methyl methacrylate in all structural units of 50% to 99% by mass, and a weight average molecular weight of 5000 to 50000.
- the photosensitive colored resin composition according to the present invention contains an alkali-soluble resin having an acid value exceeding 50 mgKOH/g and a non-reactive resin having an acid value of 7 mgKOH/g to 50 mgKOH/g.
- the content of the structural unit derived from methyl methacrylate is 50% by mass to 99% by mass in all the structural units, and the weight average molecular weight is 5000 to 50000, so that generation of development residue is suppressed even in low-temperature heat treatment. , and a colored layer having a good pattern shape can be formed.
- the action of the combination ensures the developability of the unexposed areas.
- the lower portion of the resin composition layer in the exposed area is less likely to flow during development, and undercutting of the cross section after development can be suppressed.
- the specific non-reactive resin used in the present invention is selected so as to have the specific acid value, structural unit and weight average molecular weight. Therefore, when combined with an alkali-soluble resin having a specific acid value or higher, development residue can be suppressed.
- the photosensitive colored resin composition according to the present invention can suppress the generation of development residues even in low-temperature heat treatment, and can form a colored layer with a good pattern shape. It can be suitably used for a cured film. That is, the photosensitive colored resin composition according to the present invention can be suitably used for a cured film directly formed on a device substrate having an organic light-emitting device.
- the photosensitive colored resin composition according to the present invention is used for a cured film formed adjacent to or via at least one layer on an organic light-emitting element, an external color formed on a substrate such as a glass substrate Compared to a display device in which a filter is attached to an organic light-emitting element, a display device that is thinner and more flexible can be manufactured.
- a color filter as an alternative to a polarizing plate for suppressing external light reflection It can also be used as
- the photosensitive colored resin composition according to the present invention contains at least a colorant, an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and a solvent, and the present invention It may contain other components as long as the effects of the above are not impaired.
- a colorant an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and a solvent
- the present invention It may contain other components as long as the effects of the above are not impaired.
- Each component of the photosensitive colored resin composition according to the present invention will be described in detail below.
- the coloring material is not particularly limited as long as it can develop a desired color when the colored layer of the color filter is formed, and various organic pigments, inorganic pigments, dispersible dyes, and dyes Salt-forming compounds and the like can be used alone or in combination of two or more.
- organic pigments are preferably used because of their high color developability and high heat resistance. Examples of organic pigments include compounds classified as pigments in the Color Index (C.I.; published by The Society of Dyers and Colorists). .) numbered ones can be mentioned.
- the inorganic pigments include titanium oxide, barium sulfate, calcium carbonate, zinc white, lead sulfate, yellow lead, zinc yellow, red iron oxide (III), cadmium red, ultramarine blue, Prussian blue, oxide Chromium green, cobalt green, amber, titanium black, synthetic iron black, carbon black and the like can be mentioned.
- a black pigment having high light-shielding properties is blended in the ink.
- a black pigment with high light shielding properties for example, an inorganic pigment such as carbon black or triiron tetroxide, or an organic pigment such as cyanine black can be used.
- the dispersible dyes include dyes that are made dispersible by adding various substituents to the dye or by using the dye in combination with a solvent having low solubility.
- the salt-forming compound of the dye refers to a compound in which the dye forms a salt with a counterion. Examples thereof include a salt-forming compound of a basic dye and an acid, and a salt-forming compound of an acid dye and a base, which are soluble in solvents. It also includes a lake pigment obtained by insolubilizing the dye in a solvent using a known lake formation (chlorination) technique.
- a coloring material containing at least one selected from dyes and salt-forming compounds of dyes is used in combination with the dispersant of the present invention to improve the dispersibility and dispersion stability of the coloring material. can be done.
- the dye can be appropriately selected from conventionally known dyes.
- examples of such dyes include azo dyes, metal complex salt azo dyes, anthraquinone dyes, triphenylmethane dyes, xanthene dyes, cyanine dyes, naphthoquinone dyes, quinoneimine dyes, methine dyes, and phthalocyanine dyes.
- azo dyes metal complex salt azo dyes
- anthraquinone dyes triphenylmethane dyes
- xanthene dyes cyanine dyes
- naphthoquinone dyes naphthoquinone dyes
- quinoneimine dyes methine dyes
- phthalocyanine dyes a guideline
- the coloring material is at least one selected from the group consisting of diketopyrrolopyrrole pigments, quinophthalone pigments, copper phthalocyanine pigments, zinc phthalocyanine pigments, quinophthalone dyes, coumarin dyes, cyanine dyes, and salt-forming compounds of these dyes.
- the effect of suppressing the sublimation or precipitation of the colorant due to the use of the dispersant is high, and it is preferable in that a colored layer with high brightness can be formed.
- the coloring material contains at least one selected from the group consisting of diketopyrrolopyrrole pigments, quinophthalone pigments, copper phthalocyanine pigments, zinc phthalocyanine pigments, and quinophthalone dyes.
- diketopyrrolopyrrole pigments include C.I. I. Pigment Red 254, 255, 264, 272, 291, and diketopyrrolopyrrole pigments represented by the following general formula (i), among which C.I. I. Pigment Red 254, 272, 291, and at least one selected from diketopyrrolopyrrole pigments in which R 21 and R 22 in the following general formula (i) are each a 4-bromophenyl group are preferred.
- R 51 and R 52 are each independently a 4-chlorophenyl group or a 4-bromophenyl group.
- Examples of quinophthalone pigments include C.I. I. Pigment Yellow 138 and the like.
- Examples of copper phthalocyanine pigments include C.I. I. Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, C.I. I. Pigment Green 7, 36 and the like, among which C.I. I. Pigment Blue 15:6 is preferred.
- Examples of zinc phthalocyanine pigments include C.I. I. Pigment Green 58, 59 and the like.
- Examples of quinophthalone dyes include C.I. I. Disperse Yellow 54, 64, 67, 134, 149, 160, C.I. I. Solvent Yellow 114, 157 and the like, among which C.I. I. Disperse Yellow 54 is preferred.
- the average primary particle size of the colorant used in the present invention is such that when it is formed into a cured film, it can suppress external light reflection and transmit desired light from the light emitting element to suppress the decrease in luminance of the display device. It is not particularly limited as long as it is possible, and although it varies depending on the type of coloring material used, it is preferably in the range of 10 nm to 100 nm, more preferably 15 nm to 60 nm. When the average primary particle size of the colorant is in the above range, the display device provided with the cured film produced using the photosensitive colored resin composition according to the present invention can suppress reflection of external light and has high contrast. and can be of high quality.
- the average dispersed particle size of the colorant in the photosensitive colored resin composition varies depending on the type of colorant used, but is preferably in the range of 10 nm to 100 nm, and preferably in the range of 15 nm to 60 nm. is more preferred.
- the average dispersed particle size of the colorant in the photosensitive colored resin composition is the dispersed particle size of the colorant particles dispersed in the dispersion medium containing at least a solvent, and is measured by a laser light scattering particle size distribution meter. It is a thing.
- the solvent used in the photosensitive colored resin composition is diluted appropriately to a concentration that can be measured by a laser light scattering particle size distribution meter (for example, 1000 times), and measured at 23° C. by a dynamic light scattering method using a laser light scattering particle size distribution analyzer (eg, Nanotrack particle size distribution analyzer UPA-EX150 manufactured by Nikkiso Co., Ltd.).
- the average distribution particle size here is the volume average particle size.
- the coloring material used in the present invention can be produced by known methods such as recrystallization and solvent salt milling. Alternatively, a commercially available coloring material may be used after undergoing fine processing.
- the content of the coloring material in the photosensitive colored resin composition according to the present invention is not particularly limited.
- the content of the coloring material from the viewpoint of dispersibility and dispersion stability, relative to the total solid content of the photosensitive colored resin composition, for example preferably 3 wt% to 65 wt%, more preferably 4 wt% to 60 It is within the range of % by mass. If it is at least the above lower limit, the cured film when the photosensitive colored resin composition is applied to a predetermined film thickness (usually 1.0 ⁇ m to 5.0 ⁇ m, for example, 3.0 ⁇ m) has sufficient color density. It's easy to do.
- substrate can be obtained.
- the content of the coloring material is, for example, preferably 3% by mass to 50% by mass, more preferably 4% by mass, relative to the total solid content of the photosensitive colored resin composition. % to 40% by mass.
- the solid content refers to all substances other than the solvent, which will be described later, and includes monomers and the like dissolved in the solvent.
- the alkali-soluble resin used in the present invention has an acid value of more than 50 mgKOH/g, is a resin having an acidic group, acts as a binder resin, and is soluble in an alkaline developer used for pattern formation. It can be appropriately selected and used from among them.
- Preferred alkali-soluble resins in the present invention are, specifically, (meth)acrylic resins such as (meth)acrylic copolymers having a carboxy group and styrene-(meth)acrylic copolymers having a carboxy group, Epoxy (meth)acrylate resins having a carboxyl group and the like are included.
- (meth)acrylic resins such as (meth)acrylic copolymers having a carboxy group and styrene-(meth)acrylic copolymers having a carboxy group
- Epoxy (meth)acrylate resins having a carboxyl group and the like are included.
- particularly preferred are reactive alkali-soluble resins having a carboxy group in the side chain and a reactive group in the side chain. This is because the film strength of the cured film formed by containing the reactive group is improved.
- the reactive group includes at least one selected from the group consisting of ethylenically unsaturated bond-containing groups, epoxy
- (Meth)acrylic copolymers having a structural unit having a carboxyl group, and (meth)acrylic resins such as styrene-(meth)acrylic copolymers having a carboxyl group are, for example, carboxyl group-containing ethylenic It is a (co)polymer obtained by (co)polymerizing a saturated monomer and optionally other copolymerizable monomers by a known method.
- Carboxy group-containing ethylenically unsaturated monomers include, for example, (meth)acrylic acid, vinyl benzoic acid, maleic acid, maleic acid monoalkyl ester, fumaric acid, itaconic acid, crotonic acid, cinnamic acid, and acrylic acid dimer. be done. Also, addition reaction products of monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate and cyclic anhydrides such as maleic anhydride, phthalic anhydride and cyclohexanedicarboxylic anhydride, ⁇ -carboxy-polycaprolactone Mono (meth) acrylate and the like can also be used.
- Anhydride-containing monomers such as maleic anhydride, itaconic anhydride, and citraconic anhydride may also be used as precursors of the carboxy group.
- (meth)acrylic acid is particularly preferable from the viewpoint of copolymerizability, cost, solubility, glass transition temperature, and the like.
- the alkali-soluble resin preferably further has a hydrocarbon ring from the viewpoint of excellent adhesion of the colored layer.
- the present inventors have found that the presence of a hydrocarbon ring, which is a bulky group, in the alkali-soluble resin suppresses the solvent resistance of the resulting colored layer, particularly swelling of the colored layer. Although the action is not clear, the presence of bulky hydrocarbon rings in the colored layer suppresses the movement of molecules in the colored layer, which increases the strength of the coating film and suppresses swelling due to solvents.
- hydrocarbon rings include cyclic aliphatic hydrocarbon rings which may have substituents, aromatic rings which may have substituents, and combinations thereof, and hydrocarbon rings may have a substituent such as a carbonyl group, a carboxy group, an oxycarbonyl group or an amide group.
- hydrocarbon rings may have a substituent such as a carbonyl group, a carboxy group, an oxycarbonyl group or an amide group.
- hydrocarbon rings include aliphatic hydrocarbons such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, norbornane, tricyclo[5.2.1.0(2,6)]decane (dicyclopentane), and adamantane.
- Aromatic rings such as benzene, naphthalene, anthracene, phenanthrene, and fluorene; chain polycyclic rings such as biphenyl, terphenyl, diphenylmethane, triphenylmethane, and stilbene; cardo structures represented by the following chemical formula (ii); be done.
- the alkali-soluble resin preferably has a maleimide structure represented by the following general formula (iii).
- RM is an optionally substituted hydrocarbon ring.
- the alkali-soluble resin has a maleimide structure represented by the general formula (iii), it has a nitrogen atom in the hydrocarbon ring, so that it has very good compatibility with the dispersant of the present invention, and the effect of suppressing development residue is excellent. improves.
- Specific examples of the optionally substituted hydrocarbon ring in RM of the general formula (iii) are the same as the specific examples of the hydrocarbon ring described above.
- the heat resistance and adhesiveness of the colored layer are improved, and the brightness of the obtained colored layer is also preferably improved.
- the curability of the colored layer is improved, and the solvent resistance (NMP swelling suppression) is improved, which is particularly preferable.
- the alkali-soluble resin used in the present invention using a (meth)acrylic copolymer having a structural unit having a hydrocarbon ring separately from a structural unit having a carboxy group can adjust the amount of each structural unit. It is preferable from the viewpoint that it is easy to increase the amount of the structural unit having the hydrocarbon ring and the function of the structural unit can be easily improved.
- the (meth)acrylic copolymer having a structural unit having a carboxyl group and the above hydrocarbon ring may use an ethylenically unsaturated monomer having a hydrocarbon ring as the above-mentioned "other copolymerizable monomer".
- ethylenically unsaturated monomers having a hydrocarbon ring examples include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxy Ethyl (meth) acrylate, styrene, etc., and from the point that the cross-sectional shape of the colored layer after development is maintained even in heat treatment, cyclohexyl (meth) acrylate, dicyclopentanyl (meth) acrylate, adamantyl (Meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate and styrene are preferred.
- a method for introducing an ethylenically unsaturated bond-containing group into an alkali-soluble resin may be appropriately selected from conventionally known methods. For example, a method in which a compound having both an epoxy group and an ethylenically unsaturated bond in the molecule, such as glycidyl (meth)acrylate, is added to the carboxyl group of the alkali-soluble resin to introduce an ethylenically unsaturated bond into the side chain.
- a structural unit having a hydroxyl group is introduced into a copolymer, a compound having an isocyanate group and an ethylenically unsaturated bond is added to the molecule, and an ethylenically unsaturated bond is introduced into the side chain. etc.
- the alkali-soluble resin used in the present invention may further contain other structural units such as a structural unit having an ester group such as methyl (meth)acrylate and ethyl (meth)acrylate.
- a structural unit having an ester group functions not only as a component that suppresses the alkali solubility of the photosensitive colored resin composition, but also as a component that improves the solubility in a solvent and the solvent re-solubility.
- the alkali-soluble resin used in the present invention is a (meth)acrylic copolymer and a styrene-(meth)acrylic copolymer having a structural unit having a carboxy group and a structural unit having a hydrocarbon ring ( It is preferably a meth)acrylic resin, and a (meth)acrylic copolymer and styrene having a structural unit having a carboxy group, a structural unit having a hydrocarbon ring, and a structural unit having an ethylenically unsaturated bond - (Meth)acrylic resins such as (meth)acrylic copolymers are more preferred.
- the alkali-soluble resin can be made into an alkali-soluble resin with desired performance by appropriately adjusting the charging amount of each structural unit.
- the amount of the carboxyl group-containing ethylenically unsaturated monomer to be charged is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total amount of the monomers in order to obtain a good pattern.
- the amount of the carboxyl group-containing ethylenically unsaturated monomer charged is preferably 50% by mass or less, and 40% by mass or less relative to the total amount of the monomer.
- the resulting coating film has sufficient solubility in an alkaline developer, and the proportion of the carboxy group containing ethylenically unsaturated monomer is at the above upper limit. If it is below, the formed pattern tends not to come off from the substrate and the film roughening on the pattern surface tends not to occur during development with an alkaline developer.
- (meth)acrylic copolymers and styrene-(meth)acrylic copolymers having structural units having ethylenically unsaturated bonds in side chains which are more preferably used as alkali-soluble resins
- the compound having both an epoxy group and an ethylenically unsaturated bond is preferably 10% by mass to 95% by mass with respect to the charged amount of the carboxyl group-containing ethylenically unsaturated monomer, and 15% by mass to 90% by mass. % by mass is more preferred.
- the weight average molecular weight (Mw) of the alkali-soluble resin such as the carboxy group-containing copolymer is preferably 3,000 or more, more preferably 5,000 or more, from the viewpoint of the binder function after curing. It is preferably 30,000 or less, more preferably 20,000 or less, from the viewpoint of pattern formability during development.
- the weight average molecular weight (Mw) in the present invention can be measured by Shodex GPC System-21H using polystyrene as a standard substance and THF as an eluent.
- the epoxy (meth)acrylate resin having a carboxy group is not particularly limited, but epoxy (meth) obtained by reacting a reaction product of an epoxy compound and an unsaturated group-containing monocarboxylic acid with an acid anhydride.
- Acrylate compounds are suitable.
- Epoxy compounds, unsaturated group-containing monocarboxylic acids, and acid anhydrides can be appropriately selected from known ones and used. For example, the description in paragraphs 0226 to 0240 of Japanese Patent No. 6911365 can be referred to and used as appropriate.
- epoxy (meth)acrylate resins having a carboxy group examples include polymers of epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, or epoxy group-containing (meth)acrylates and other ethylenically unsaturated monomers.
- Epoxy (meth)acrylate resins having a carboxy group may be used alone or in combination of two or more.
- an alkali-soluble resin having an acid value of more than 50 mgKOH/g is selected and used.
- the alkali-soluble resin preferably has an acid value of 60 mgKOH/g or more and 300 mgKOH/g or less, especially 70 mgKOH/g or more, in terms of developability with an alkaline aqueous solution used in the developer and adhesion to the substrate. It is preferably 200 mgKOH/g or less.
- the upper limit of the acid value may be 150 mgKOH/g or less, 120 mgKOH/g or less, or 100 mgKOH/g or less.
- the acid value in the present invention can be measured according to JIS K 0070:1992.
- the ethylenically unsaturated bond equivalent when the side chain of the alkali-soluble resin has an ethylenically unsaturated bond improves the film strength of the cured film, improves solvent resistance and development resistance, and has excellent adhesion to the substrate. From the viewpoint of obtaining such effects, it is preferably in the range of 100 to 2000, and particularly preferably in the range of 140 to 1500. If the ethylenically unsaturated bond equivalent is 2000 or less, the solvent resistance, development resistance and adhesion are excellent. Also, if it is 100 or more, the ratio of other structural units such as structural units having a carboxy group and structural units having a hydrocarbon ring can be relatively increased, so that excellent developability and heat resistance can be obtained.
- the ethylenically unsaturated bond equivalent is the weight average molecular weight per mole of the ethylenically unsaturated bond in the alkali-soluble resin, and is represented by the following formula (1).
- Ethylenically unsaturated bond equivalent (g / mol) W (g) / M (mol) (In formula (1), W represents the mass (g) of the alkali-soluble resin, and M represents the number of moles (mol) of ethylenically unsaturated bonds contained in the alkali-soluble resin W (g).)
- the ethylenically unsaturated bond equivalent is obtained, for example, by measuring the number of ethylenically unsaturated bonds contained per 1 g of the alkali-soluble resin in accordance with the iodine value test method described in JIS K 0070: 1992. can be calculated.
- the alkali-soluble resins used in the photosensitive colored resin composition may be used singly or in combination of two or more.
- the content of the alkali-soluble resin is not particularly limited, but is preferably 5% to 60% by mass, more preferably 10% to 40% by mass, based on the total solid content of the photosensitive colored resin composition. Within range. When the content of the alkali-soluble resin is at least the above lower limit, sufficient alkali developability is obtained, and when the content of the alkali-soluble resin is at most the above upper limit, film roughness and pattern chipping during development are prevented. can be suppressed.
- the non-reactive resin used in the present invention has an acid value of 7 mgKOH/g to 50 mgKOH/g, and the content of structural units derived from methyl methacrylate is 50% to 99% by mass of all structural units, It has a weight average molecular weight of 5,000 to 50,000.
- the non-reactive resin used in the present invention is basically a resin that does not have at least one reactive group selected from the group consisting of an ethylenically unsaturated bond-containing group, an epoxy group, an oxetane group, and a blocked isocyanate group. is.
- the non-reactive resin used in the present invention has an acid value of 7 mgKOH/g or more, preferably 20 mgKOH/g or more, more preferably 30 mgKOH/g or more, from the viewpoint of suppressing development residues.
- the non-reactive resin used in the present invention has an acid value of 50 mgKOH/g or less, may be 47 mgKOH/g or less, preferably 45 mgKOH/g or less, more preferably 45 mgKOH/g or less, from the viewpoint of improving the undercut shape. is 40 mgKOH/g or less.
- the non-reactive resin used in the present invention may be a copolymer containing structural units derived from methyl methacrylate.
- the content of structural units derived from methyl methacrylate in all structural units is 50% by mass or more, preferably 90% by mass or more, from the viewpoint of improving the undercut shape. Yes, more preferably 92% by mass or more.
- the content of structural units derived from methyl methacrylate is 99% by mass or less, preferably 98% by mass or less, and more preferably 97% by mass or less, based on all structural units, from the viewpoint of suppressing development residues.
- the non-reactive resin used in the present invention may be a (meth)acrylic copolymer containing a structural unit derived from an ethylenically unsaturated monomer copolymerizable with a structural unit derived from methyl methacrylate. It may be a (meth)acrylic copolymer having a structural unit derived from methyl and a structural unit having an acidic group, and a (meth)acrylic copolymer containing a structural unit derived from methyl methacrylate and a structural unit having a carboxy group. It may be a system copolymer. Examples of structural units having a carboxy group include structural units derived from carboxy group-containing ethylenically unsaturated monomers.
- the carboxy group-containing ethylenically unsaturated monomer may be the same as the carboxy group-containing ethylenically unsaturated monomers listed in the alkali-soluble resin.
- Acrylic acid is particularly preferred.
- the content of the structural unit having a carboxy group may be appropriately adjusted according to the acid value, and is selected from the range of 1% by mass to 10% by mass, preferably 2% by mass or more, more preferably 2% by mass or more, of all the structural units. is 3% by mass or more, preferably 9% by mass or less, and more preferably 8% by mass or less.
- the non-reactive resin used in the present invention is a structural unit derived from methyl methacrylate and a structural unit having an acidic group, as well as a structural unit derived from methyl methacrylate, as long as the effects of the present invention are not impaired. It may have other constitutional units derived from polymerizable ethylenically unsaturated monomers. Other copolymerizable ethylenically unsaturated monomers may be the same as the ethylenically unsaturated monomers exemplified for the alkali-soluble resin. Among other copolymerizable ethylenically unsaturated monomers, those having no alkali-soluble substituents are preferable from the viewpoint of suppressing undercut shapes.
- copolymerizable ethylenically unsaturated monomers include, for example, ethyl methacrylate, butyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, cyclohexyl methacrylate, dicyclopentanyl methacrylate, isobornyl methacrylate, tetrahydrofurfuryl methacrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, dimethylaminomethyl methacrylate, diethylaminoethyl methacrylate, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane ethoxysilane, 3-methacryloxypropyltriethoxysilane, and the like.
- Other structural units may be used in combination of two or more.
- the total content of structural units derived from methyl methacrylate and structural units having an acidic group may be 100% by mass of all structural units, and the structural units derived from methyl methacrylate and The total content of structural units having a carboxy group may be 100% by mass in all structural units.
- the weight average molecular weight (Mw) of the non-reactive resin used in the present invention is 5,000 or more, preferably 7,000 or more, more preferably 9,000 or more from the viewpoint of improving the undercut shape.
- the weight average molecular weight (Mw) is 50,000 or less, preferably 30,000 or less, more preferably 20,000 or less, from the viewpoint of suppressing development residue.
- the non-reactive resin used in the present invention can be prepared in the same manner as the alkali-soluble resin.
- the non-reactive resin used in the present invention may have a glass transition temperature (Tg) exceeding 0°C, 20°C or higher, or 50°C or higher.
- the glass transition temperature (Tg) of the alkali-soluble resin is measured using differential scanning calorimetry (DSC) (for example, EXSTAR DSC 7020 manufactured by SII Nanotechnology) according to the method described in JIS K7121. be able to.
- DSC differential scanning calorimetry
- EXSTAR DSC 7020 manufactured by SII Nanotechnology the method described in JIS K7121.
- the peak area that is, the peak having the largest area of the portion projecting from the base line of the obtained chart is taken as the representative value of the glass transition temperature.
- the glass transition temperature (Tg) of the copolymer can be calculated by the following formula and used as a guideline.
- Tgi is the glass transition temperature (absolute temperature) of the homopolymer of the i-th monomer.
- Tgi homopolymer glass transition temperature value of each monomer, the value in Polymer Handbook (3rd Edition) (J. Brandrup, EHImmergut (Wiley-Interscience, 1989)) can be adopted.
- the non-reactive resin used in the photosensitive colored resin composition may be used singly or in combination of two or more.
- the content of the non-reactive resin may be appropriately selected and used, but from the viewpoint of improving the undercut shape, it is preferably 1% by mass or more relative to the total solid content of the photosensitive colored resin composition. It is preferably 2% by mass or more, more preferably 4% by mass or more.
- the content of the non-reactive resin is preferably 20% by mass or less, more preferably 15% by mass or less, more preferably 15% by mass or less, based on the total solid content of the photosensitive colored resin composition. It is 12% by mass or less.
- the content of the non-reactive resin used in the photosensitive colored resin composition is preferably It is 1% by mass or more, more preferably 5% by mass or more, and still more preferably 10% by mass or more.
- the content of the non-reactive resin is preferably 80% by mass or less, more preferably 70% by mass, based on the total content of the reactive alkali-soluble resin and the non-reactive resin. % or less, more preferably 60 mass % or less.
- photopolymerizable compound used in the photosensitive colored resin composition examples include compounds having a photopolymerizable group in the molecule.
- the photopolymerizable group is not particularly limited as long as it can be polymerized by a photoinitiator, and includes ethylenically unsaturated bond-containing groups such as vinyl, allyl, acryloyl and methacryloyl groups. are mentioned.
- an acryloyl group or a methacryloyl group is preferably used from the viewpoint of ultraviolet curability.
- the photopolymerizable compound from the viewpoint of curability, it is preferable to contain a compound having two or more photopolymerizable groups in one molecule, and a compound having three or more photopolymerizable groups in one molecule is contained. is more preferable.
- a compound having two or more ethylenically unsaturated bonds is preferably used, and a polyfunctional (meth)acrylate having two or more acryloyl groups or methacryloyl groups is particularly preferable.
- a polyfunctional (meth)acrylate may be appropriately selected from among conventionally known ones and used. Specific examples include those described in JP-A-2013-029832.
- polyfunctional (meth)acrylates may be used singly or in combination of two or more. Further, when excellent photocurability (high sensitivity) is required for the photosensitive colored resin composition of the present invention, the polyfunctional (meth)acrylate has three polymerizable ethylenically unsaturated bonds (three Functionality) or more is preferable, and poly(meth)acrylates of trihydric or higher polyhydric alcohols and their dicarboxylic acid-modified products are preferable.
- trimethylolpropane tri(meth)acrylate penta Erythritol tri(meth)acrylate, succinic acid-modified pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol penta (Meth)acrylate modified with succinic acid, dipentaerythritol hexa(meth)acrylate and the like are preferred.
- the content of the photopolymerizable compound used in the photosensitive colored resin composition is not particularly limited, but relative to the total solid content of the photosensitive colored resin composition, for example preferably 5% by mass to 60% by mass, More preferably, it is within the range of 10% by mass to 40% by mass. If the content of the photopolymerizable compound is at least the above lower limit, photocuring will proceed sufficiently, and the exposed portion will be able to suppress elution during development. Adequate alkali developability.
- photoinitiator used in the photosensitive colored resin composition of the present invention one or a combination of two or more of conventionally known various photoinitiators can be used.
- photoinitiators include aromatic ketones, benzoin ethers, halomethyloxadiazole compounds, ⁇ -aminoketones, biimidazoles, N,N-dimethylaminobenzophenone, halomethyl-S-triazine compounds, and thioxanthone. , oxime esters, and the like.
- a photoinitiator a conventionally known photoinitiator can be used, and examples thereof include the photoinitiator described in WO 2018/062105.
- Examples of the oxime ester photoinitiator used in the present invention include 1,2-octadione-1-[4-(phenylthio)phenyl]-,2-(o-benzoyloxime), ethanone, 1-[ 9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), JP-A-2000-80068, JP-A-2001-233842, special table 2010-527339, JP 2010-527338, JP 2013-041153, WO 2015/152153, JP 2010-256891, among the oxime ester photoinitiators described in It can be selected as appropriate.
- the oxime ester photoinitiator is a compound represented by the following general formula (A) and the following general formula ( It preferably contains at least one compound represented by B).
- R 1 and R 2 each independently represent R 11 , OR 11 , COR 11 , SR 11 , CONR 12 R 13 or CN;
- R 11 , R 12 and R 13 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or an arylalkyl group having 7 to 30 carbon atoms or 2 to 20 carbon atoms.
- R 21 , R 22 and R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or an arylalkyl group having 7 to 30 carbon atoms or 2 to 20 carbon atoms.
- R 21 , R 22 and R 23 represents a heterocyclic group of hydrogen atoms in the groups represented by R 21 , R 22 and R 23 may be further substituted with a hydroxyl group, a nitro group, CN, a halogen atom, or a carboxy group;
- the alkylene portions of the groups represented by R 11 , R 12 , R 13 , R 21 , R 22 and R 23 are -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 -, -SCO-, -COS-, -OCS- or -CSO- may contain 1 to 5 oxygen atoms not adjacent to each other,
- R 24 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or a
- R 3 may be The hydrogen atoms of the group represented by R 3 may further be R 21 , OR 21 , COR 21 , SR 21 , NR 22 R 23 , CONR 22 R 23 , —NR 22 —OR 23 , —NCOR 22 —OCOR 23 , NR 22 COR 21 , OCOR 21 , COOR 21 , SCOR 21 , OCSR 21 , COSR 21 , CSOR 21 , a hydroxyl group, a nitro group, CN, or optionally substituted with a halogen atom
- R 4 , R 5 , R 6 and R 7 are each independently R 11 , OR 11 , SR 11 , COR 14 , CONR 15 R 16 , NR 12 COR 11 , OCOR 11 , COOR 14 , SCOR 11 , OCSR 11 , COSR 14 , CSOR 11 , a hydroxyl group, CN or a halogen atom, R 4 and R 5 , R 6
- R 8 is R 11 , OR 11 , SR 11 , COR 11 , CONR 12 R 13 , NR 12 COR 11 , OCOR 11 , COOR 11 , SCOR 11 , OCSR 11 , COSR 11 , CSOR 11 represents a hydroxyl group, CN or a halogen atom, k represents 0 or 1; )
- X 1 , X 3 and X 6 each independently represent R 41 , OR 41 , COR 41 , SR 41 , CONR 42 R 43 or CN;
- X 2 has 1 to represents an alkyl group having 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or a heterocyclic group having 2 to 20 carbon atoms, and
- X 4 and X 5 each independently represent R 41 , OR 41 , SR 41 , COR 41 , CONR 42 R 43 , NR 42 COR 41 , OCOR 41 , COOR 41 , SCOR 41 , COSR 41 , COSR 41 , CSOR 41 , CN, halogen atom or hydroxyl group;
- R 41 , R 42 and R 43 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylal
- R 51 , R 52 and R 53 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or an arylalkyl group having 7 to 30 carbon atoms or 2 to 20 carbon atoms.
- R 54 represents a heterocyclic group of hydrogen atoms of the groups represented by R 51 , R 52 and R 53 may be further substituted with a hydroxyl group, a nitro group, CN, a halogen atom or a carboxy group;
- the alkylene portions of the groups represented by R 41 , R 42 , R 43 , X 2 , R 51 , R 52 and R 53 are -O-, -S-, -COO-, -OCO-, -NR 54 - , -NR 54 CO-, -NR 54 COO-, -OCONR 54 -, -SCO-, -COS-, -OCS- or -CSO-, even if 1 to 5 oxygen atoms are not adjacent Often, R 54 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms or a heterocycl
- the oxime ester compound represented by the general formula (A) includes geometric isomers due to the double bond of the oxime, but these are not to be distinguished. That is, in the present specification, the compound represented by the general formula (A), and the compound represented by the following general formula (A'), which is a preferred form of the compound described later, and the exemplary compounds thereof are a mixture of both or either It represents one or the other, and is not limited to the structure showing the isomer.
- alkyl group 1 to 20 carbon atoms represented by R 3 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 21 , R 22 , R 23 and R 24 in the above general formula (A)
- alkyl group examples include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, amyl, isoamyl, t-amyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, t- octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, icosyl, cyclopentyl, cyclopenty
- Examples of the aryl group having 6 to 30 carbon atoms represented by R 3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 in the general formula (A) include phenyl , tolyl, xylyl, ethylphenyl, naphthyl, anthryl, phenanthrenyl, phenyl substituted with one or more of the above alkyl groups, biphenylyl, naphthyl, anthryl, and the like.
- Examples of arylalkyl groups having 7 to 30 carbon atoms represented by R 3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 in general formula (A) include: benzyl, ⁇ -methylbenzyl, ⁇ , ⁇ -dimethylbenzyl, phenylethyl and the like.
- heterocyclic groups having 2 to 20 carbon atoms represented by R 3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 in the general formula (A) include , pyridyl, pyrimidyl, furyl, thienyl, tetrahydrofuryl, dioxolanyl, benzoxazol-2-yl, tetrahydropyranyl, pyrrolidyl, imidazolidyl, pyrazolidyl, thiazolidyl, isothiazolidyl, oxazolidyl, isoxazolidyl, piperidyl, piperazyl, morpholinyl, etc.
- the rings that can be formed by R 4 and R 5 , R 5 and R 6 , R 6 and R 7 , R 3 and R 7 and R 3 and R 8 together include: Preferred examples include 5- to 7-membered rings such as cyclopentane ring, cyclohexane ring, cyclopentene ring, benzene ring, piperidine ring, morpholine ring, lactone ring and lactam ring.
- Halogen atoms represented by R 4 , R 5 , R 6 , R 7 and R 8 in general formula (A), and R 3 , R 11 and R 12 in general formula (A) , R 13 , R 21 , R 22 and R 23 may be substituted with fluorine, chlorine, bromine and iodine.
- the alkylene moieties of the groups represented by R 11 , R 12 , R 13 , R 21 , R 22 and R 23 in the above general formula (A) are -O-, -S-, -COO-, -OCO -, -NR 24 -, -NR 24 CO-, -NR 24 COO- , -OCONR 24 -, -SCO-, -COS-, -OCS- or -CSO-, 1 to 1 under the condition that oxygen atoms are not adjacent to each other; It may contain 5 divalent groups, and the divalent groups contained at this time may be one or more groups, and in the case of groups that can be contained continuously, 2 or more may be contained continuously. .
- alkyl (alkylene) moieties of the groups represented by R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 in the general formula (A) have branched side chains. may be a cyclic alkyl.
- R 3 is an optionally condensed aromatic ring or compounds represented by the following general formula (A') have high sensitivity and can be manufactured is preferred because it is easy to
- R 31 , R 32 , R 33 , R 34 and R 35 are each independently R 11 , OR 11 , SR 11 , COR 11 , CONR 15 R 16 , NR 12 COR 11 , OCOR 11 , COOR 14 , SCOR 11 , OCSR 11 , COSR 14 , CSOR 11 , hydroxyl group , a nitro group, CN or a halogen atom, and R 31 and R 32 , R 32 and R 33 , R 33 and R 34 and R 34 and R 35 may each form a ring together.
- rings formed by R 31 and R 32 , R 32 and R 33 , R 33 and R 34 and R 34 and R 35 together include R 4 and R 5 , R 5 and R 6 and R 6 and R 7 and R 3 and R 7 and R 3 and R 8 together may be formed by the same rings as those mentioned above.
- R 1 is an alkyl group having 1 to 12 carbon atoms or an arylalkyl group having 7 to 15 carbon atoms
- R 11 is an aryl group having 6 to 12 carbon atoms
- 1 carbon atom is preferable because of its high solvent solubility
- an alkyl group of R 2 is preferably a methyl group, an ethyl group or a phenyl group because of its high reactivity
- R 4 to R 7 is a hydrogen atom or a cyano A group, particularly a hydrogen atom, is preferred for ease of synthesis.
- a hydrogen atom as R 8 is preferred for ease of synthesis.
- k is preferably 1 for high sensitivity.
- R 31 to R 35 is a nitro group, CN, a halogen atom, or COR 11
- R 11 is an aryl group having 6 to 12 carbon atoms or an alkyl group having 1 to 8 carbon atoms.
- High sensitivity is preferred, and at least one of R 31 to R 35 is more preferably a nitro group, CN, a halogen atom, or COPh (where Ph is a phenyl group), and R 33 is a nitro group, CN, or a halogen atom. Atoms, or COPh, are particularly preferred.
- Preferred specific examples of the compound represented by the general formula (A) include the following compounds.
- the oxime ester compound represented by the general formula (B) also has geometric isomers due to the double bond of the oxime, but these are not distinguished. That is, in the present specification, the compound represented by the general formula (B) and its exemplified compounds represent a mixture of both or either one, and are not limited to structures showing isomers.
- the alkyl group having 1 to 20 carbon atoms represented by X 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 may be The same as the alkyl group having 1 to 20 carbon atoms in (A) can be mentioned.
- the aryl group having 6 to 30 carbon atoms represented by X 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 in the general formula (B) is Examples thereof include the same aryl groups having 6 to 30 carbon atoms in (A).
- the arylalkyl group having 7 to 30 carbon atoms represented by X 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 in the general formula (B) includes Examples thereof include the same arylalkyl groups having 7 to 30 carbon atoms in formula (A).
- the heterocyclic group having 2 to 20 carbon atoms represented by X 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 in the general formula (B) includes Examples thereof include the same heterocyclic groups having 2 to 20 carbon atoms in formula (A).
- examples of the halogen atom in the general formula (B) include the same halogen atoms as the halogen atoms in the general formula (A).
- alkylene moieties of the groups represented by R 41 , R 42 , R 43 , X 2 , R 51 , R 52 and R 53 in the above general formula (B) are -O-, -S-, -COO- , -OCO-, -NR 54 -, -NR 54 CO-, -NR 54 COO- , -OCONR 54 -, -SCO-, -COS-, -OCS- or -CSO- under conditions where oxygen atoms are not adjacent to each other may contain 1 to 5, and the divalent groups contained at this time may be one or more groups, and in the case of groups that can be contained continuously, two or more are contained continuously. may
- X 1 is more preferably a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, from the viewpoint of sensitivity, solubility and compatibility.
- Alkyl groups having 1 to 10 carbon atoms such as t-butyl, n-amyl, isoamyl, t-amyl, n-hexyl and 2-ethylhexyl groups, and 5 carbon atoms such as cyclopentyl and cyclohexyl groups cyclic alkyl groups which may have up to 10 side chains, or groups such as methoxymethyl, ethoxymethyl, ethoxyethyl, 2-(1-methoxypropyl) and 2-(1-ethoxypropyl) groups It is an alkyl group having 2 to 10 carbon atoms and having one ether bond in a methylene chain, more preferably an alkyl group having 1 to 10 carbon atoms such as methyl, ethyl and 2-ethylhexyl.
- X 2 , X 3 and X 6 are each independently from the viewpoint of sensitivity, solubility and compatibility, and particularly preferably methyl group, ethyl group, n-propyl group and isopropyl alkyl groups having 1 to 6 carbon atoms such as groups, n-butyl groups, isobutyl groups, t-butyl groups, n-amyl groups, isoamyl groups, t-amyl groups and n-hexyl groups, cyclopentyl groups and cyclohexyl groups
- a cyclic alkyl group having 5 to 6 carbon atoms such as, or a carbon number such as methoxymethyl group, ethoxymethyl group, ethoxyethyl group, 2-(1-methoxypropyl) group and 2-(1-ethoxypropyl) group is an alkyl group having 2 to 6 carbon atoms and one ether bond in the methylene chain, more preferably an
- X 3 and X 6 are each independently preferably an alkyl group having 1 to 6 carbon atoms in terms of sensitivity, solubility and compatibility. From the viewpoint of sensitivity, solubility and compatibility, X2 is more preferably an alkyl group having 2 to 6 carbon atoms and having one ether bond in the methylene chain.
- X 4 and X 5 are each independently from the viewpoint of sensitivity, solubility and compatibility, and particularly preferably hydrogen, or a methyl group, an ethyl group, an n-propyl group, C1-C6 alkyl groups such as isopropyl, n-butyl, isobutyl, t-butyl, n-amyl, isoamyl, t-amyl and n-hexyl groups.
- a and b are each independently an integer of 0 to 3, may be an integer of 0 to 1, or may be 0;
- Preferred specific examples of the compound represented by the general formula (B) include the following compounds.
- the total content of the photoinitiator used in the photosensitive colored resin composition of the present invention is not particularly limited as long as the effect of the present invention is not impaired, relative to the total solid content of the photosensitive colored resin composition, It is preferably in the range of 0.1% by mass to 15.0% by mass, more preferably in the range of 1.0% by mass to 10.0% by mass. If the content is at least the above lower limit, photocuring will proceed sufficiently, and the solvent resistance and substrate adhesion will tend to be good. easy to form patterns.
- the total content of at least one of the compound represented by the general formula (A) and the compound represented by the general formula (B) is a cured film having good substrate adhesion and solvent resistance even in low-temperature heat treatment.
- the total amount of the photoinitiator is preferably 30.0% by mass or more, more preferably 50.0% by mass or more, still more preferably 70.0% by mass or more, and 100% by mass can be
- the solvent used in the present invention is not particularly limited as long as it does not react with each component in the photosensitive colored resin composition and is capable of dissolving or dispersing them.
- a solvent can be used individually or in combination of 2 or more types.
- Specific examples of solvents include alcohol solvents such as methyl alcohol, ethyl alcohol, N-propyl alcohol, i-propyl alcohol, methoxy alcohol and ethoxy alcohol; carbitol solvents such as methoxyethoxyethanol and ethoxyethoxyethanol; ethyl acetate, butyl acetate, methyl methoxypropionate, ethyl methoxypropionate, ethyl ethoxypropionate, ethyl lactate, methyl hydroxypropionate, ethyl hydroxypropionate, n-butyl acetate, isobutyl acetate, isobutyl butyrate, n-butyl butyrate, ester solvents such
- glycol ether acetate-based solvents examples include propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, butyl carbitol acetate (BCA), 3-methoxy-3-methyl-1-butyl acetate, ethyl ethoxypropionate, ethyl lactate, and one or more selected from the group consisting of 3-methoxybutyl acetate, from the viewpoint of solubility of other components and applicability.
- BCA butyl carbitol acetate
- 3-methoxy-3-methyl-1-butyl acetate ethyl ethoxypropionate
- ethyl lactate examples include one or more selected from the group consisting of 3-methoxybutyl acetate, from the viewpoint of solubility of other components and applicability.
- the content of the solvent may be appropriately set within a range in which the colored layer can be formed with high precision.
- the content of the solvent is usually in the range of preferably 55% by mass to 95% by mass, more preferably 65% by mass to 88% by mass, based on the total amount of the photosensitive colored resin composition containing the solvent. When the content of the solvent is within the above range, excellent applicability can be obtained.
- a dispersant when the colorant is dispersed, a dispersant may be further included from the viewpoint of colorant dispersibility and colorant dispersion stability.
- the dispersant can be appropriately selected and used from conventionally known dispersants.
- the dispersing agent for example, a cationic, anionic, nonionic, amphoteric, silicone or fluorine surfactant can be used.
- surfactants polymer dispersants are preferred because they can be uniformly and finely dispersed.
- polymer dispersants include (meth)acrylate copolymer dispersants; polyurethanes; unsaturated polyamides; polysiloxanes; long-chain polyaminoamide phosphates; amides obtained by reaction with free carboxyl group-containing polyesters and their bases); polyallylamine derivatives (polyallylamine and polyesters having free carboxyl groups, polyamides, or cocondensates of esters and amides (polyesteramides) (a reaction product obtained by reacting with one or more compounds selected from the compounds of ), and the like.
- polymer dispersants include (meth)acrylate copolymer dispersants; polyurethanes; unsaturated polyamides; polysiloxanes; long-chain polyaminoamide phosphates; amides obtained by reaction with free carboxyl group-containing polyesters and their bases); polyallylamine derivatives (polyallylamine and polyesters having free carboxyl groups, polyamides, or cocondensates of esters and
- (meth)acrylate copolymer-based dispersant it is preferable to use a (meth)acrylate copolymer-based dispersant as the dispersant, since solvent resistance tends to be improved even with low-temperature heat treatment.
- (Meth) acrylate copolymer-based dispersant has good compatibility with the alkali-soluble resin, the non-reactive resin, the photopolymerizable compound and the photoinitiator, so that the initiator can be uniformly dispersed in the colored layer. As the colored layer hardens uniformly, the amount of unreacted components decreases and the internal stress of the colored layer decreases, so it is presumed that the colored layer changes less when immersed in a solvent.
- the (meth)acrylate copolymer-based dispersant refers to a dispersant that is a copolymer and contains at least a (meth)acrylate-derived structural unit.
- the (meth)acrylate copolymer-based dispersant is preferably a copolymer containing a structural unit that functions as a coloring material adsorption site and a structural unit that functions as a solvent affinity site, and functions as a solvent affinity site. It is preferable that at least a (meth)acrylate-derived structural unit is included in the structural units to be formed.
- Examples of structural units that function as colorant adsorption sites include structural units derived from ethylenically unsaturated monomers copolymerizable with structural units derived from (meth)acrylate.
- the coloring material adsorption site may be a structural unit derived from an ethylenically unsaturated monomer containing an acidic group, or a structural unit derived from an ethylenically unsaturated monomer containing a basic group.
- a structural unit represented by the following general formula (I) is preferable from the viewpoint of excellent dispersibility.
- R 71 is a hydrogen atom or a methyl group
- a 1 is a divalent linking group
- R 72 and R 73 are each independently a hydrogen atom, or a hydrocarbon which may contain a hetero atom. group, and R 72 and R 73 may combine with each other to form a ring structure.
- a 1 is a divalent linking group.
- the divalent linking group for example, a linear, branched or cyclic alkylene group, a linear, branched or cyclic alkylene group having a hydroxyl group, an arylene group, -CONH- group, -COO- group, -NHCOO- groups, ether groups (--O--groups), thioether groups (--S--groups), and combinations thereof.
- the bonding direction of the divalent linking group is arbitrary.
- a 1 in the general formula (I) is preferably a divalent linking group containing a -CONH- group or a -COO- group, and a -CONH- group or a -COO- group.
- an alkylene group having 1 to 10 carbon atoms are more preferable.
- Examples of the hydrocarbon group in the hydrocarbon group optionally containing a heteroatom for R 72 and R 73 include an alkyl group, an aralkyl group and an aryl group.
- Examples of the alkyl group include methyl group, ethyl group, propyl group, butyl group, isopropyl group, tert-butyl group, 2-ethylhexyl group, cyclopentyl group, cyclohexyl group and the like, and the number of carbon atoms in the alkyl group is 1. to 18 are preferable, and among them, a methyl group or an ethyl group is more preferable.
- the aralkyl group includes, for example, a benzyl group, a phenethyl group, a naphthylmethyl group, a biphenylmethyl group and the like.
- the number of carbon atoms in the aralkyl group is preferably 7-20, more preferably 7-14.
- Aryl groups include phenyl, biphenyl, naphthyl, tolyl, and xylyl groups.
- the number of carbon atoms in the aryl group is preferably 6-24, more preferably 6-12.
- the number of carbon atoms of the substituent is not included in the preferable number of carbon atoms.
- a hydrocarbon group containing a heteroatom has a structure in which a carbon atom in the hydrocarbon group is replaced with a heteroatom, or a structure in which a hydrogen atom in the hydrocarbon group is replaced by a substituent containing a heteroatom.
- the heteroatom that the hydrocarbon group may contain include an oxygen atom, a nitrogen atom, a sulfur atom, a silicon atom and the like.
- hydrogen atoms in the hydrocarbon group may be substituted with halogen atoms such as fluorine, chlorine and bromine atoms.
- R 72 and R 73 are bonded to each other to form a ring structure means that R 72 and R 73 form a ring structure via a nitrogen atom.
- the ring structure formed by R72 and R73 may contain a heteroatom.
- the ring structure is not particularly limited, examples thereof include pyrrolidine ring, piperidine ring, morpholine ring and the like.
- R 72 and R 73 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, or R 72 and R 73 are bonded to form a pyrrolidine ring, piperidine It preferably forms a ring or a morpholine ring.
- Examples of monomers that derive structural units represented by the general formula (I) include dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminoethyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and the like.
- Alkyl group-substituted amino group-containing (meth)acrylates, alkyl group-substituted amino group-containing (meth)acrylamides such as dimethylaminoethyl (meth)acrylamide, dimethylaminopropyl (meth)acrylamide, and the like can be mentioned.
- dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylamide can be preferably used in terms of improving dispersibility and dispersion stability.
- the structural unit represented by formula (I) may consist of one type, or may contain two or more types of structural units.
- the structural unit functioning as the coloring material adsorption site is selected from the group consisting of at least part of the nitrogen site possessed by the structural unit represented by the general formula (I), an organic acid compound, and a halogenated hydrocarbon. At least one of them may form a salt (hereinafter, such a copolymer may be referred to as a salt-type copolymer).
- a compound represented by the following general formula (1) and a compound represented by the following general formula (3) are preferable.
- at least one compound selected from the group consisting of the organic acid compound and the halogenated hydrocarbon is preferably one or more compounds selected from the group consisting of the following general formulas (1) to (3). can.
- R a is a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl group which may have a substituent or a benzyl group, or -O- Represents R e
- R e is a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl group which may have a substituent or a benzyl group, or a C 1 to 4 represents a (meth)acryloyl group via an alkylene group.
- R b , R b′ , and R b′′ each independently represent a hydrogen atom, an acidic group or an ester group thereof, or a substituent.
- a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms a vinyl group which may have a substituent, a phenyl group which may have a substituent or a benzyl group, or -O- R f represents an optionally substituted linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group optionally having a substituent, a substituted may be a phenyl group or a benzyl group, or a (meth)acryloyl group via an alkylene group having 1 to 4 carbon atoms, and X represents a chlorine atom, a bromine atom, or an iodine atom.
- R c and R d are each independently a hydrogen atom, a hydroxyl group, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, an optionally substituted phenyl group or a benzyl group, Alternatively, —O—R e , where R e is a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, an optionally substituted phenyl group or a benzyl group, or a carbon number represents a (meth)acryloyl group via 1 to 4 alkylene groups, provided that at least one of R c and R d contains a carbon atom.
- the organic acid compound is an acidic organic phosphorus compound such as phenylphosphonic acid or phenylphosphinic acid from the viewpoint of excellent dispersibility and dispersion stability of the coloring material.
- the organic acid compound used in such a dispersant include, for example, organic acid compounds described in JP-A-2012-236882 and the like as suitable ones.
- the halogenated hydrocarbon is preferably at least one selected from allyl halides such as allyl bromide and benzyl chloride, and aralkyl halides, from the viewpoint of excellent dispersibility and dispersion stability of the coloring material.
- the content of at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with the terminal nitrogen moiety of the structural unit represented by general formula (I). Therefore, the total of at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons is 0 for the terminal nitrogen portion of the structural unit represented by general formula (I) It is preferably 0.01 mol or more, more preferably 0.05 mol or more, even more preferably 0.1 mol or more, and particularly preferably 0.2 mol or more. When it is at least the above lower limit, the effect of improving the dispersibility of the coloring material by salt formation is likely to be obtained.
- At least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons may be used singly or in combination of two or more. When combining two or more, the total content is preferably within the above range.
- the salt-type copolymer As a method for preparing the salt-type copolymer, at least one selected from the group consisting of the organic acid compound and the halogenated hydrocarbon is added to a solvent in which the copolymer before salt formation is dissolved or dispersed, and the mixture is stirred. and a method of heating if necessary.
- the terminal nitrogen portion of the structural unit represented by the general formula (I) of the copolymer and at least one selected from the group consisting of the organic acid compound and the halogenated hydrocarbon form a salt. and the ratio thereof can be confirmed by a known method such as NMR.
- the copolymer having the structural unit represented by the general formula (I) has the structural unit represented by the general formula (I), and the graft polymer chain ( A graft copolymer having a meth)acrylate-derived structural unit, and a block having an A block containing a structural unit represented by the general formula (I) and a B block containing a (meth)acrylate-derived structural unit is more preferably at least one of copolymers.
- a graft polymer chain having a structural unit derived from (meth)acrylate a conventionally known structure can be appropriately selected and used.
- graft copolymer and the salt-type graft copolymer described in WO2021/006077 may be used.
- block copolymer as the B block containing a structural unit derived from (meth)acrylate, a conventionally known structure can be appropriately selected and used.
- block copolymers and salt-type block copolymers described in WO2016/104493 may be used.
- the A block containing the structural unit represented by the general formula (I) and the B block containing the structural unit derived from the carboxy group-containing monomer and the (meth)acrylate-derived structural unit and from the group consisting of at least part of the nitrogen moiety of the structural unit represented by the general formula (I) of the block copolymer, an organic acid compound, and a halogenated hydrocarbon Contains at least one salt-type block copolymer formed with at least one selected salt, and the block copolymer and at least one of the salt-type block copolymers have an acid value of 1 mgKOH/g to 18 mgKOH.
- the B block in this case contains a (meth)acrylate-derived structural unit as an essential component, and may be the same as the B block of WO 2016/104493.
- the (meth)acrylate copolymer containing the structural unit represented by the general formula (I) is a copolymer having an amine value of 40 mgKOH/g to 120 mgKOH/g. It is preferable from the viewpoint of improving brightness and contrast without depositing foreign substances. When the amine value is within the above range, the viscosity stability over time and heat resistance are excellent, and alkali developability and solvent re-solubility are also excellent.
- the (meth)acrylate copolymer containing the structural unit represented by the general formula (I) preferably has an amine value of 80 mgKOH/g or more, particularly 90 mgKOH/g or more. is more preferable.
- the amine value of the (meth)acrylate copolymer containing the structural unit represented by the general formula (I) is preferably 110 mgKOH/g or less, and 105 mgKOH/g.
- the following are more preferable.
- the amine value refers to the number of mg of potassium hydroxide equivalent to perchloric acid required to neutralize the amine component contained in 1 g of the sample, and can be measured by the method defined in JIS-K7237. When measured by this method, even if the amino group forms a salt with the organic acid compound in the dispersant, the organic acid compound usually dissociates, so the block copolymer itself used as the dispersant can be measured.
- the content ratio (mol%) of each structural unit in the copolymer in the dispersant can be obtained from the amount of raw materials charged at the time of production, and can be measured using an analyzer such as NMR. Also, the structure of the dispersant can be measured using NMR, various mass spectrometry, and the like. In addition, if necessary, the dispersant is decomposed by thermal decomposition or the like, and the resulting decomposition product is subjected to high performance liquid chromatography, gas chromatograph mass spectrometer, NMR, elemental analysis, XPS / ESCA, TOF-SIMS, etc. can ask.
- the content of the dispersant is not particularly limited as long as it is selected so as to be excellent in the dispersibility and dispersion stability of the coloring material, but in the photosensitive colored resin composition
- it is preferably in the range of 2% by mass to 30% by mass, more preferably 3% by mass to 25% by mass, based on the total solid content.
- the dispersibility and dispersion stability of the coloring material are excellent, and the storage stability of the photosensitive colored resin composition is excellent.
- developability will become favorable.
- the content of the dispersant is, for example, preferably 2% by mass to 25% by mass, more preferably 2% by mass to 25% by mass, based on the total solid content of the photosensitive colored resin composition. It is within the range of 3% by mass to 20% by mass.
- the photosensitive colored resin composition of the present invention preferably further contains at least one of a polyfunctional epoxy compound and a polyfunctional blocked isocyanate compound from the viewpoint of improving solvent resistance after low-temperature heat treatment.
- a polyfunctional epoxy compound is a compound having two or more epoxy groups in one molecule.
- An epoxy group means a group containing a three-membered cyclic ether structure, and includes an alicyclic epoxy group.
- Epoxy groups include an oxiranyl group and a 3,4-epoxycyclohexyl group. Some or all of the hydrogen atoms in these epoxy groups may be substituted with substituents such as alkyl groups.
- polyfunctional epoxy compounds include bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, hydrogenated bisphenol F diglycidyl ether, and hydrogenated bisphenol AD diglycidyl ether.
- Polyfunctional epoxy compounds may be used alone or in combination of two or more. Among them, 1,2-epoxy-4-(2-oxiranyl)cyclohexane of 2,2-bis(hydroxymethyl)-1-butanol An adduct is preferred because it tends to improve solvent resistance after low-temperature heat treatment.
- a polyfunctional blocked isocyanate compound is a compound having two or more blocked isocyanate groups in one molecule.
- a blocked isocyanate group is a group obtained by blocking an isocyanate group with a blocking agent.
- the polyfunctional blocked isocyanate compound remains stable at around room temperature, and the blocking agent is dissociated by heat treatment to regenerate the active isocyanate group. Obtained by reacting a compound with a blocking agent.
- polyfunctional isocyanate compounds include 2,4- and/or 2,6-tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, p-phenylene diisocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, 3, aromatic diisocyanates such as 3′-dimethyldiphenyl-4,4′-diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, dicyclohexylmethane-4,4′-diisocyanate, trans-1,4-cyclohexyl diisocyanate and norbornane diisocyanate; diethylene Diisocyanate, tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4 and/or (2,4,4)-trimethylhexamethylene diisocyanate, lysine diisocyanate, cyclohex
- heterocyclic diisocyanates, etc., and diisocyanates such as carbodiimide-modified, isocyanurate-modified, and biuret-modified products of these diisocyanate compounds.
- triphenylmethane triisocyanate 1-methylbenzol-2,4,6-triisocyanate, dimethyltriphenylmethane tetraisocyanate, N,N′,N′′-tri(1-isocyanatohexyl)isocyanuric acid, lysine triisocyanate , tris(phenylisocyanate) thiophosphate, 4,4′,4′′-triisocyanate-2,5-dimethoxyphenylamine, 1,3,5-triisocyanatocyclohexane, 1,3,5-tris(isocyanatomethyl ) cyclohexane, etc.
- Trifunctional or higher isocyanate compounds such as carbodiimide-modified, isocyanurate-modified and biuret-modified products of these isocyanate compounds can be mentioned. These can be used singly or in combination of two or more. Among these isocyanate compounds, alicyclic diisocyanates and aliphatic diisocyanates are more preferable from the viewpoint of transparency.
- the blocking agent known blocking agents can be appropriately selected and used. Active methylene compounds such as acetylacetone and acetoacetate esters (methyl acetoacetate, ethyl acetoacetate, etc.), 3,5-dimethylpyrazole and the like are preferably used.
- the content of at least one of the polyfunctional epoxy compound and the polyfunctional blocked isocyanate compound is usually 3% to 30% by mass, preferably 5% to 20% by mass, based on the total solid content of the photosensitive colored resin composition. It is within the range of % by mass. If it is at least the above lower limit, it is easy to improve the solvent resistance and substrate adhesion after low-temperature heat treatment. On the other hand, if it is the above upper limit or less, the photosensitive colored resin composition of the present invention tends to have good developability.
- the photosensitive colored resin composition of the present invention preferably further contains a thiol compound from the viewpoint of improving solvent resistance after low-temperature heat treatment and substrate adhesion.
- thiol compounds include monofunctional thiol compounds having one thiol group in one molecule and polyfunctional thiol compounds having two or more thiol groups in one molecule. From the viewpoint of suppressing line width shift and improving substrate adhesion, it is more preferable to use a monofunctional thiol compound having one thiol group.
- Examples of monofunctional thiol compounds include 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, 2-mercapto-5-methoxybenzothiazole, 2-mercapto-5-methoxybenzimidazole, 3-mercapto propionic acid, methyl 3-mercaptopropionate, ethyl 3-mercaptopropionate, octyl 3-mercaptopropionate and the like.
- polyfunctional thiol compounds include 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2, 4,6(1H,3H,5H)-trione, trimethylolpropane tris (3-mercaptopropionate), pentaerythritol tetrakis (3-mercaptobutyrate), pentaerythritol tetrakis (3-mercaptopropionate), di pentaerythritol hexakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate) and the like.
- the thiol compound may be used alone or in combination of two or more. Among them, 2-mercaptobenzoxazole or 2-mercaptobenzothiazole improves solvent resistance and substrate adhesion after low-temperature heat treatment. It is preferable from the point of view.
- the content of the thiol compound is usually in the range of 0.5% by mass to 10% by mass, preferably 1% by mass to 5% by mass, based on the total solid content of the photosensitive colored resin composition. If it is at least the above lower limit, the solvent resistance after low-temperature heat treatment and substrate adhesion are excellent. On the other hand, if it is at most the above upper limit, the photosensitive colored resin composition of the present invention tends to have good developability and suppressed line width shift.
- the photosensitive colored resin composition of the present invention may further contain various additives.
- additives include antioxidants, polymerization terminators, chain transfer agents, leveling agents, plasticizers, surfactants, antifoaming agents, silane coupling agents, ultraviolet absorbers, adhesion promoters, and the like.
- specific examples of surfactants and plasticizers include those described in JP-A-2013-029832.
- the photosensitive colored resin composition of the present invention preferably further contains an antioxidant from the viewpoint of suppressing the line width shift amount of the cured film.
- the photosensitive colored resin composition of the present invention for example, by containing an antioxidant in combination with the compound represented by the general formula (A), excessive without impairing the curability when forming a cured film Since the radical chain reaction can be controlled, when forming a fine line pattern, the linearity is further improved, and the ability to form the fine line pattern according to the design of the mask line width is improved. In addition, the heat resistance can be improved, and the decrease in luminance after exposure and post-baking can be suppressed, so the luminance can be improved.
- the antioxidant used in the present invention is not particularly limited, and may be appropriately selected from those conventionally known.
- antioxidants include hindered phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, hydrazine-based antioxidants, and the like. It is preferable to use a hindered phenol-based antioxidant from the viewpoint of improving the ability to form a fine line pattern according to the design of the line width and from the viewpoint of heat resistance. It may also be a latent antioxidant as described in WO 2014/021023.
- Hindered phenol-based antioxidants include, for example, pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (trade name: trade name: IRGANOX1010, manufactured by BASF), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanurate (trade name: Irganox 3114, manufactured by BASF), 2,4,6-tris(4-hydroxy-3 ,5-di-tert-butylbenzyl)mesitylene (trade name: Irganox 1330, manufactured by BASF), 2,2′-methylenebis(6-tert-butyl-4-methylphenol) (trade name: Sumilizer MDP-S, Sumitomo Chemical), 6,6′-thiobis(2-tert-butyl-4-methylphenol) (trade name: Irganox 1081, manufactured by BASF), 3,5-di-
- pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: IRGANOX1010, manufactured by BASF) is preferable from the viewpoint of heat resistance and light resistance. .
- the content of the antioxidant is usually 0.1% by mass to 10.0% by mass, preferably 0.5% by mass to 5.0% by mass, based on the total solid content of the photosensitive colored resin composition. Within range. If it is at least the above lower limit, the ability to form a fine line pattern as designed with a mask line width is improved, and the heat resistance is excellent. On the other hand, if it is below the said upper limit, it will be easy to make the photosensitive colored resin composition of this invention into a highly sensitive photosensitive colored resin composition.
- silane coupling agents examples include KBM-502, KBM-503, KBE-502, KBE-503, KBM-5103, KBM-903, KBE-903, KBM573, KBM-403, KBE-402, KBE-403 , KBM-303, KBM-802, KBM-803, KBE-9007, X-12-967C (manufactured by Shin-Etsu Silicone Co., Ltd.) and the like.
- KBM-502, KBM-503, KBE-502, KBE-503 and KBM-5103 having a methacrylic group or an acrylic group are preferable from the viewpoint of adhesion to SiN substrates.
- the content of the silane coupling agent is usually 0.05% by mass to 10.0% by mass, preferably 0.1% by mass to 5.0% by mass, based on the total solid content in the photosensitive colored resin composition. %. If it is more than the said lower limit and below the said upper limit, the board
- the method for producing a photosensitive colored resin composition of the present invention comprises a coloring material, an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, a solvent, and various additive components optionally used. can be prepared by mixing with using a known mixing means.
- the photosensitive colored resin composition of the present invention is, for example, a colorant, an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, a dispersant, a solvent, and various kinds of materials used as desired.
- the method for preparing the resin composition includes, for example, (1) First, a coloring material and a dispersant are added to a solvent to prepare a coloring material dispersion, and the dispersion is (2) a method of mixing an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and various additive components optionally used; (2) a coloring material and a dispersing agent in a solvent; , a method of simultaneously adding and mixing an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and optionally various additive components; (3) a dispersant in a solvent; A method of adding and mixing an alkali-soluble resin, a non-reactive resin, a photopolymerizable compound, a photoinitiator, and various additive components that are optionally used, and then adding and dispersing a coloring material; (4) A coloring material, a
- the above methods (1) and (4) are preferable because they can effectively prevent the aggregation of the colorant and uniformly disperse the colorant.
- the dispersant may be removed and prepared by the above method (2), (3) or (4).
- the method for preparing the colorant dispersion can be appropriately selected from conventionally known dispersion methods. For example, (1) a dispersant is mixed with a solvent in advance and stirred to prepare a dispersant solution, and then an organic acid compound is mixed as necessary to form a salt between the amino group of the dispersant and the organic acid compound.
- a method of mixing this with a coloring material and, if necessary, other components and dispersing using a known stirrer or disperser (2) mixing and stirring a dispersant in a solvent to prepare a dispersant solution; , a coloring material and, if necessary, an organic acid compound, and if necessary, other components are mixed and dispersed using a known stirrer or disperser; (3) a dispersant is mixed with a solvent and stirred; , Prepare a dispersant solution, then mix the coloring material and other components as necessary, make a dispersion using a known stirrer or disperser, and then add an organic acid compound as necessary. methods and the like.
- dispersing machines for dispersing include roll mills such as two-roll and three-roll roll mills, ball mills such as ball mills and vibrating ball mills, bead mills such as paint conditioners, continuous disk-type bead mills, and continuous annular-type bead mills.
- the diameter of the beads used is preferably 0.03 mm to 2.00 mm, more preferably 0.10 mm to 1.0 mm.
- the photosensitive colored resin composition according to the present invention can suppress the generation of development residues even in low-temperature heat treatment, and can form a colored layer with a good pattern shape, so it can be suitably used for color filters.
- it can be suitably used for low-temperature heat treatment applications such as 130° C. or less, further 100° C. or less or 90° C. or less in which a color filter is directly formed on a substrate on which an element having low heat resistance such as an organic light-emitting element is formed. It can be suitably used for a cured film formed on an organic light-emitting device.
- the photosensitive colored resin composition according to the present invention can be used for a cured film formed on an organic light emitting device, it is suitable for forming a colored cured film as a substitute for a circularly polarizing plate having an external light reflection suppressing effect. Used.
- the cured film of the photosensitive colored resin composition according to the present invention is used in place of the circularly polarizing plate, it can be a display device that does not contain a polarizing plate, so the photosensitive colored resin composition according to the present invention is , is suitably used for display devices that do not contain a polarizing plate.
- the photosensitive colored resin composition according to the present invention is a photosensitive colored resin composition used for a cured film formed on an organic light-emitting element, it can be It is suitable for use in organic light-emitting display devices with improved flexibility.
- the cured product according to the present invention is a cured product of the photosensitive colored resin composition according to the present invention.
- the cured product according to the present invention forms a coating film of the photosensitive colored resin composition according to the present invention, and after drying the coating film, exposure, and if necessary development, obtained by heat treatment be able to.
- the methods of forming, exposing, developing, and heat-treating the coating film may be, for example, the same methods as those used in the formation of the colored layer provided in the color filter according to the present invention, which will be described later.
- the cured product according to the present invention has good solvent resistance and good pattern shape even when the heat treatment is performed at a low temperature of 130° C. or lower, 100° C. or lower, or 90° C. or lower.
- the cured product according to the present invention has good solvent resistance even when subjected to low-temperature heat treatment, and has a good pattern shape. Used.
- the color filter according to the present invention is a color filter comprising at least a substrate and a colored layer provided on the substrate, wherein at least one of the colored layers is the photosensitive colored resin composition according to the present invention. It is a hardened material.
- FIG. 1 is a schematic cross-sectional view showing an example of the color filter of the present invention.
- the color filter 10 of the present invention has a substrate 1, a light shielding portion 2 and a colored layer 3. As shown in FIG.
- At least one of the colored layers used in the color filter of the present invention is a colored layer that is a cured product of the photosensitive colored resin composition according to the present invention.
- the colored layer is usually formed in the opening of the light shielding part on the substrate, which will be described later, and is usually composed of colored patterns of three or more colors.
- the arrangement of the colored layers is not particularly limited, and may be a general arrangement such as a stripe type, mosaic type, triangle type, four-pixel arrangement type, or the like. Moreover, the width, area, etc. of the colored layer can be arbitrarily set.
- the thickness of the colored layer can be appropriately controlled by adjusting the coating method, solid content concentration and viscosity of the photosensitive colored resin composition, and is preferably in the range of 1 to 5 ⁇ m.
- the colored layer can be formed, for example, by the following method.
- a coating method such as a spray coating method, a dip coating method, a bar coating method, a roll coating method, a spin coating method, or a die coating method.
- the spin coating method and the die coating method can be preferably used.
- After drying the wet coating film using a hot plate, oven, etc. it is exposed through a mask of a predetermined pattern to photopolymerize the alkali-soluble resin and the polyfunctional monomer, etc. to cure. It is used as a coating film.
- Light sources used for exposure include, for example, ultraviolet light from low-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, electron beams, and the like.
- the amount of exposure is appropriately adjusted depending on the light source used, the thickness of the coating film, and the like.
- heat treatment may be performed.
- the heating conditions are appropriately selected according to the mixing ratio of each component in the photosensitive colored resin composition to be used, the thickness of the coating film, and the like.
- a coating film is formed in a desired pattern by developing with a developer to dissolve and remove the unexposed portions.
- a solution obtained by dissolving an alkali in water or a water-soluble solvent is usually used.
- An appropriate amount of a surfactant or the like may be added to this alkaline solution.
- a general method can be adopted as the developing method.
- the developing solution is usually washed and the cured coating film of the photosensitive colored resin composition is dried to form a colored layer.
- the heating conditions are not particularly limited, and are appropriately selected according to the application of the coating film.
- the heat treatment in the manufacturing process for forming the colored layer directly on the element substrate is preferably performed at 30° C. or higher and 100° C. or lower, more preferably 35° C. or higher and 95° C. or lower, and 40° C. or higher and 90° C. or lower. It is even more preferable to do so.
- the colored layer is formed in a desired pattern by a conventionally known method for forming a patterned coating film such as an inkjet method. After the formation, the film is exposed to light and a photopolymerization reaction of a photopolymerizable compound or the like is performed to form a cured coating film. In the same manner as described above, heat treatment may be performed in order to promote the polymerization reaction after exposure.
- the light-shielding portion in the color filter of the present invention is formed in a pattern on a substrate, which will be described later, and can be the same as those used as light-shielding portions in general color filters.
- the pattern shape of the light shielding portion is not particularly limited, and examples thereof include a stripe shape, a matrix shape, and the like.
- the light shielding portion may be a metal thin film of chromium or the like formed by a sputtering method, a vacuum deposition method, or the like.
- the light-shielding portion may be a resin layer containing light-shielding particles such as carbon fine particles, metal oxides, inorganic pigments, or organic pigments in a resin binder.
- a method of patterning by development using a photosensitive resist a method of patterning using an inkjet ink containing light-shielding particles, a method of thermally transferring a photosensitive resist, and the like are available. be.
- the film thickness of the light-shielding portion is set to about 0.2 to 0.4 ⁇ m in the case of a metal thin film, and is set to about 0.5 to 2 ⁇ m in the case of a black pigment dispersed or dissolved in a binder resin. be done.
- a transparent substrate, a silicon substrate, and a transparent substrate or a silicon substrate on which an aluminum, silver, silver/copper/palladium alloy thin film or the like is formed are used.
- Other color filter layers, resin layers, transistors such as TFTs, circuits, and the like may be formed on these substrates.
- the substrate may be an element substrate such as an organic light emitting element which will be described later.
- the transparent substrate in the color filter of the present invention is not particularly limited as long as it is transparent to visible light, and transparent substrates used in general color filters can be used. Specifically, transparent rigid materials such as quartz glass, alkali-free glass, and synthetic quartz plates, or transparent flexible materials such as transparent resin films, optical resin plates, and flexible glass. material.
- transparent resin films and optical resin plates examples include polyethylene terephthalate (PET) films, polyimide films, and polycarbonate films. It is preferably used.
- PET polyethylene terephthalate
- the thickness of the transparent substrate is not particularly limited, a thickness of about 100 ⁇ m to 1 mm, for example, can be used depending on the application of the color filter of the present invention.
- the color filter of the present invention may be formed with, for example, an overcoat layer, a transparent electrode layer, an alignment film, columnar spacers, etc., in addition to the above substrate, light shielding portion and colored layer.
- the color filter of the present invention can also be used as a substitute for a circularly polarizing plate that prevents reflection of external light.
- Display Device A display device according to the present invention includes the color filter according to the present invention.
- the configuration of the display device is not particularly limited, and can be appropriately selected from conventionally known display devices, such as liquid crystal display devices and organic light-emitting display devices.
- FIG. 2 is a schematic diagram showing an example of the liquid crystal display device of the present invention.
- a liquid crystal display device 40 of the present invention includes a color filter 10, a counter substrate 20 having a TFT array substrate and the like, and a liquid crystal layer formed between the color filter 10 and the counter substrate 20.
- the liquid crystal display device of the present invention is not limited to the configuration shown in FIG. 2, and may have a known configuration as a liquid crystal display device generally using color filters.
- the driving method of the liquid crystal display device of the present invention is not particularly limited, and a driving method generally used for liquid crystal display devices can be adopted. Examples of such driving methods include the TN method, the IPS method, the OCB method, and the MVA method. Any of these methods can be suitably used in the present invention. Also, the counter substrate can be appropriately selected and used according to the driving method of the liquid crystal display device of the present invention. Further, as the liquid crystal constituting the liquid crystal layer, various liquid crystals having different dielectric anisotropy and mixtures thereof can be used according to the driving method of the liquid crystal display device of the present invention.
- a method for forming the liquid crystal layer a method generally used as a method for manufacturing a liquid crystal cell can be used, and examples thereof include a vacuum injection method and a liquid crystal dropping method. After the liquid crystal layer is formed by the above method, the liquid crystal cell is gradually cooled to room temperature, thereby aligning the enclosed liquid crystal.
- FIG. 3 is a schematic diagram showing an example of the organic light-emitting display device of the present invention.
- the organic light emitting diode display 100 of the present invention has an organic light emitting element 80 and a sealing layer 90 formed on a substrate 50, and a color filter 10 is formed thereon.
- the substrate 50 may be a flexible substrate on which a TFT is formed.
- the color filter 10 may be a color filter substituting for a circular polarizer.
- a transparent anode 71, a hole injection layer 72, a hole transport layer 73, a light emitting layer 74, an electron injection layer 75, and a cathode 76 are sequentially formed on the substrate 50. and the like.
- the transparent anode 71, the hole injection layer 72, the hole transport layer 73, the light emitting layer 74, the electron injection layer 75, the cathode 76, and other structures in the organic light emitting device 80 known structures can be appropriately used.
- the sealing layer 90 can use a well-known thing suitably.
- the organic light-emitting display device 100 manufactured in this way can be applied to, for example, a passive drive type organic EL display and an active drive type organic EL display.
- the organic light-emitting display device of the present invention is not limited to the configuration shown in FIG. 3, and may have a known configuration as an organic light-emitting display device generally using color filters.
- the display device according to the present invention may have a cured film of the photosensitive colored resin composition according to the present invention on the organic light-emitting element.
- a display device according to the present invention since the cured film of the photosensitive colored resin composition according to the present invention is formed on the organic light-emitting element, an external circularly polarizing plate, An external color filter substrate is unnecessary and may be absent.
- Such a display device according to the present invention uses the photosensitive colored resin composition according to the present invention to form a cured film on the organic light-emitting element. Since it does not have a substrate that is used as an attached color filter substrate, it has improved thinness and flexibility.
- FIG. 4 is a schematic cross-sectional view showing another example of a display device having an organic light emitting device according to the present invention.
- a display device 200 according to the present invention includes an element substrate 130 having an organic light emitting element, and an external light reflection preventing film including colored cured films (109R, 109G, 109B) on the element substrate 130.
- a membrane 120 is provided, and a sealing membrane 111 is provided thereon.
- a device substrate 130 having the organic light emitting device includes a substrate 101 on which thin film transistors (TFTs) 102, which are driving devices, are arranged so as to correspond to respective sub-pixels, and a sealing film 103 is provided thereon.
- An electrode 104 (anode) corresponding to each sub-pixel and partition walls 105 partitioning each sub-pixel are provided on 103, and organic light-emitting elements (106R, 106G , 106B) are arranged, and an electrode 107 (cathode) is further provided on the organic light-emitting elements (106R, 106G, 106B).
- the element substrate 130 having the organic light emitting elements further includes a sealing layer 108 covering the organic light emitting elements from thereon.
- a display device 200 according to the present invention in FIG. 4 further includes a cover material 113 on a sealing film 111 with a transparent adhesive layer 112 interposed therebetween.
- the display device 200 according to the present invention has a known structure such as a touch sensor layer including an insulating film and a transparent electrode layer on the sealing film 111 and a hard coat layer on the touch sensor layer. may be further provided as appropriate.
- the layers of the colored cured films (109R, 109G, 109B) and the light shielding part 110 provided on the element substrate 130 having the organic light emitting element are used as the external light antireflection film 120.
- the external light antireflection film used in the present invention does not include a separate substrate such as an external circularly polarizing plate or an external color filter substrate, and can improve thinness and flexibility.
- the colors (106R, 106G, 106B) of the sub-pixels of the organic light-emitting element and the colored cured films (109R, 109G, 109B) are preferably adjusted to be of the same kind.
- the colored cured film provided on the organic light-emitting element blocks external light except for the color originally emitted by the organic light-emitting element, and does not block the light emitted by the organic light-emitting element, thereby improving the light utilization efficiency. It is possible to suppress the external light reflection without lowering it.
- the cured film of the photosensitive colored resin composition according to the present invention may be any one of the three colored cured films (109R, 109G, 109B), or may be all of them. .
- a substrate 101 used in a display device according to the present invention a thin film transistor (TFT) 102 as a driving element, a sealing film 103, an electrode 104 (anode), a partition wall 105 partitioning each sub-pixel, and an organic light-emitting element constituting a sub-pixel. (106R, 106G, 106B), the electrode 107 (cathode), etc. can be used by appropriately selecting known configurations.
- the organic light-emitting device may have known structures such as a hole injection layer, a hole transport layer, an electron injection layer, etc., in addition to the light-emitting layer.
- the sealing layer 108 on the organic EL element used in the display device according to the present invention is composed of an inorganic film, an organic film, and a multilayer film in which these are laminated. It is preferable to use a multilayer film because it has a high effect of suppressing penetration of moisture and oxygen. Specific examples thereof include a multilayer film in which an inorganic film such as a metal film, a metal oxide film, SiOx, SiON, and SiNx and an organic film are laminated.
- At least one of the colored cured films used in the display device according to the present invention is a cured film of the photosensitive colored resin composition according to the present invention.
- the colored cured film is usually formed in an opening of a light shielding part, which will be described later, on the sealing layer 108 on the organic light emitting element, and is usually composed of colored patterns of three or more colors. These may be colored patterns similar to (106R, 106G, 106B) of the sub-pixels of the organic light emitting device.
- the arrangement of the colored cured films (109R, 109G, 109B) may be, for example, a general arrangement such as a stripe type, mosaic type, triangle type, or 4-pixel arrangement type. Also, the width, area, etc.
- the thickness of the colored cured film is appropriately controlled by adjusting the coating method, solid content concentration and viscosity of the photosensitive colored resin composition, and is usually in the range of 1 ⁇ m to 5 ⁇ m.
- the light shielding part 110 used in the display device according to the present invention is usually formed in a pattern on the sealing layer 108 on the organic light emitting element, and is used as a light shielding part in a general color filter.
- the pattern shape of the light shielding portion may be appropriately selected in accordance with the shape of the colored cured film, and examples thereof include a stripe shape and a matrix shape.
- the light shielding portion may be a metal thin film of chromium or the like formed by a sputtering method, a vacuum deposition method, or the like.
- the light-shielding portion may be a resin layer containing light-shielding particles such as carbon fine particles, metal oxides, inorganic pigments, or organic pigments in a resin binder.
- a resin layer containing light-shielding particles a method of patterning by development using a photosensitive resist, a method of patterning using an inkjet ink containing light-shielding particles, a method of thermally transferring a photosensitive resist, and the like can be used. be.
- the film thickness of the light-shielding portion is set to about 0.2 ⁇ m to 0.4 ⁇ m in the case of a metal thin film, and is set to about 0.5 ⁇ m to 2 ⁇ m in the case of a black pigment dispersed or dissolved in a binder resin. be done.
- known materials can be appropriately selected and used. Also, for the transparent adhesive layer 112 provided on the sealing film 111 and the cover material 113, known materials can be appropriately selected and used. In the present invention, even when glass is used as the cover material, glass can be used as the cover material because the green cured film has good weather resistance and the reduction in transmittance is suppressed.
- the display device according to the present invention is not limited to the configuration shown in FIG. 4, and may further include the configuration of a display device having a known organic light-emitting element. .
- Method for producing a laminate of an organic light-emitting element and an anti-reflection film for external light comprises: A step of forming a coating film by applying the photosensitive colored resin composition according to the present invention on the organic light emitting device; a step of irradiating the coating film with light; A post-baking step of heating the film after the light irradiation, and By including the step of developing the film after the light irradiation, A step of forming a cured film of the photosensitive colored resin composition according to the present invention on the organic light-emitting element. Each step will be described below.
- the above-mentioned organic light-emitting element may not be applied adjacent to the organic light-emitting element, and may be applied through at least one layer.
- the electrodes 107 and the permeation of moisture and oxygen are usually further suppressed on the sub-pixels (106R, 106G, 106B) of the organic light emitting elements.
- the sealing layer 108 is provided for the purpose, it may be applied onto the organic light-emitting element through these electrodes, the sealing layer, and the like.
- the light shielding portion 110 is provided in advance on the sealing layer 108 by a known method as exemplified above, and the colored cured films (109R, 109G, 109B) are formed in the openings of the light shielding portion 110. It may be applied as follows.
- a coating means such as a die coating method, the above-described photosensitive colored resin composition of the present invention, on the organic light-emitting element to apply.
- spin coating and die coating are preferably used. Then, the wet coating film is dried using a hot plate, an oven, or the like to form a coating film.
- the obtained coating film is irradiated with light (exposure) through a mask of a predetermined pattern, and the photopolymerizable compound and, if necessary, the alkali-soluble resin, etc. are photopolymerized.
- Light sources used for exposure include, for example, ultraviolet light from low-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, electron beams, and the like. The amount of exposure is appropriately adjusted depending on the light source used, the thickness of the coating film, and the like.
- a post-baking step of heating the film after the light irradiation may be performed.
- the heating conditions may be appropriately selected according to the mixing ratio of each component in the photosensitive colored resin composition to be used, the thickness of the coating film, and the like.
- the post-baking process may be performed on the film after the light irradiation before the development process described later, after the development process, or before and after the development process.
- the heating temperature in the post-baking step is preferably 130° C. or less because the colored cured film is directly formed on the element substrate having the organic light-emitting element.
- the heating temperature is more preferably 100° C. or lower, still more preferably 90° C. or lower.
- the heating temperature may be 30° C. or higher, 35° C. or higher, or 40° C. or higher.
- the film after the light irradiation to be developed may be a film after post-baking.
- a coating film is formed in a desired pattern by developing with a developer to dissolve and remove the unexposed portions.
- a developer a solution obtained by dissolving an alkali in water or a water-soluble solvent is usually used. An appropriate amount of a surfactant or the like may be added to this alkaline solution.
- a general method can be adopted as the developing method.
- the heating temperature in this post-baking step is preferably 130° C. or less, more preferably 100° C. or less, and even more preferably 90° C. or less. .
- the heating temperature may be 30° C. or higher, 35° C. or higher, or 40° C. or higher.
- light irradiation may be additionally performed after development processing or in order to further harden the film after post-baking.
- Synthesis Example 2 Synthesis of non-reactive resin 2
- Synthesis Example 1 was carried out in the same manner as in Synthesis Example 1, except that methyl methacrylate was changed from 95% by mass to 93% by mass in all monomers, and methacrylic acid was changed from 5% by mass to 7% by mass in all monomers.
- a non-reactive resin 2 was synthesized by Table 2 shows the weight average molecular weight and acid value of the obtained non-reactive resin 2.
- Synthesis Example 3 Synthesis of non-reactive resin 3
- Synthesis Example 1 was carried out in the same manner as in Synthesis Example 1, except that methyl methacrylate was changed from 95% by mass to 99% by mass in all monomers, and methacrylic acid was changed from 5% by mass to 1% by mass in all monomers.
- a non-reactive resin 3 was synthesized by Table 2 shows the weight average molecular weight and acid value of the obtained non-reactive resin 3.
- Synthesis Example 10 Synthesis of non-reactive resin 10. Same as Synthesis Example 1 except that in Synthesis Example 1, methyl methacrylate was changed from 95% by mass in all monomers to 70% by mass in all monomers and ethyl methacrylate was changed to 25% by mass in all monomers. Then, a non-reactive resin 10 was synthesized. Table 2 shows the weight average molecular weight and acid value of the obtained non-reactive resin 10.
- Synthesis Example 11 Synthesis of non-reactive resin 11
- Synthesis Example 11 Synthesis of non-reactive resin 11
- methyl methacrylate was changed from 95% by mass in all monomers to 50% by mass in all monomers and ethyl methacrylate was changed to 45% by mass in all monomers.
- a non-reactive resin 11 was synthesized.
- Table 2 shows the weight average molecular weight and acid value of the obtained non-reactive resin 11.
- Comparative non-reactive resin c1 was synthesized in the same manner as in Synthesis Example 1, except that 95% by mass of methyl methacrylate monomer was changed to 95% by mass of butyl methacrylate monomer.
- Table 5 shows the weight average molecular weight and acid value of the obtained comparative non-reactive resin c1.
- Comparative Synthesis Example 2 Synthesis of comparative non-reactive resin c2
- a comparative non-reactive resin c2 was synthesized in the same manner as in Synthesis Example 1, except that the amount of the chain transfer agent (n-dodecylmercaptan) added was changed to 0 parts by mass.
- Table 5 shows the weight average molecular weight and acid value of the obtained comparative non-reactive resin c2.
- Comparative Synthesis Example 3 Synthesis of comparative non-reactive resin c3
- a comparative non-reactive resin c3 was synthesized in the same manner as in Synthesis Example 1, except that the amount of the chain transfer agent (n-dodecylmercaptan) added was changed to 10 parts by mass.
- Table 5 shows the weight average molecular weight and acid value of the obtained comparative non-reactive resin c3.
- Comparative Synthesis Example 4 Synthesis of comparative non-reactive resin c4
- a comparative non-reactive resin c4 was synthesized in the same manner as in Synthesis Example 1, except that the methyl methacrylate monomer was changed from 95% by mass to 100% by mass.
- Table 5 shows the weight average molecular weight and acid value of the obtained comparative non-reactive resin c4.
- EEMA 1-ethoxyethyl methacrylate
- TMSMA 2-(trimethylsilyloxy)ethyl methacrylate
- EHMA 2-ethylhexyl methacrylate
- BMA n-butyl methacrylate
- BzMA benzyl methacrylate
- MMA methyl methacrylate
- DMMA dimethylaminoethyl methacrylate
- block copolymer PGMEA solution was reprecipitated in hexane, filtered, and purified by vacuum drying to obtain block copolymer 1 (amine value: 95 mg KOH/ g, acid value 8 mgKOH/g, Tg 38°C).
- the weight average molecular weight Mw was 7,730.
- Example 1 Production of photosensitive colored resin composition R-1)
- Production of Colorant Dispersion R (1) In a 225 mL mayonnaise bottle, 72.1 parts by mass of PGMEA, 15.0 parts by mass of the alkali-soluble resin A solution of Preparation Example 1 (solid content: 40% by mass), Preparation Example 12 10.2 parts by mass of a PGMEA solution (solid content: 35% by mass) of block copolymer 1 was added and stirred. 0.4 parts by mass of phenylphosphonic acid (trade name: PPA, manufactured by Nissan Chemical Industries, Ltd.) was added thereto, and the mixture was stirred at room temperature for 30 minutes.
- PPA phenylphosphonic acid
- the block copolymer 1 is salt-formed with phenylphosphonic acid to form a salt-type block copolymer 1 .
- Examples 2 to 11 Production of photosensitive colored resin compositions R-2 to R-11
- the type and / or mass ratio of the non-reactive resin was changed, and the formula (A-2) represented Photosensitive colored resin composition R-1 except that the ratio of the oxime ester photoinitiator was the same as in Example 1 and the mass ratio of the polyfunctional monomer was changed so that the pigment concentration was the same as in Example 1.
- photosensitive colored resin compositions R-2 to R-11 were obtained.
- Example 12 to 21 Production of photosensitive colored resin compositions R-12 to R-21
- (1) Production of Colorant Dispersion Liquids R(2) to (11) A colorant dispersion was prepared in the same manner as the colorant dispersion liquid R (1), except that the type of resin was changed to alkali-soluble resin B, C, D, E, F, G, H, I, J, or K. Liquids R (2) to (11) were obtained.
- Example 22 Production of photosensitive colored resin composition R-22
- oxime ester photoinitiator represented by the formula (A-2), a fluorine-based surfactant (trade name Megafac R-08MH, DIC Corporation )), 0.1 parts by mass of a polyfunctional epoxy compound (1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, trade name EHPE3150, 10 parts by mass of Daicel Co., Ltd.) and 170.5 parts by mass of PGMEA were added to obtain a photosensitive colored resin composition R-22.
- A-2 the oxime ester photoinitiator represented by the formula (A-2), a fluorine-based surfactant (trade name Megafac R-08MH, DIC Corporation )), 0.1 parts by mass of a polyfunctional epoxy compound (1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, trade name EHPE31
- Example 23 Production of photosensitive colored resin composition R-23)
- the polyfunctional epoxy compound was changed to a polyfunctional blocked isocyanate compound (trade name Duranate MF-K60B, manufactured by Asahi Kasei Corporation) in the same manner as the photosensitive colored resin composition R-22.
- a colored resin composition R-23 was obtained.
- Example 24 Production of photosensitive colored resin composition G-1)
- Production of Colorant Dispersion G (1) In a 225 mL mayonnaise bottle, 72.1 parts by mass of PGMEA, 15 parts by mass of the alkali-soluble resin A solution (solid content: 40% by mass) of Preparation Example 1, and the block of Preparation Example 12 are mixed. 10.2 parts by mass of a PGMEA solution of copolymer 1 (solid content: 35% by mass) was added and stirred. 0.4 parts by mass of phenylphosphonic acid (trade name: PPA, manufactured by Nissan Chemical Industries, Ltd.) was added thereto, and the mixture was stirred at room temperature for 30 minutes.
- PPA phenylphosphonic acid
- Pigment Green 59 in 8.0 parts by mass and C.I. I. 5.3 parts by mass of Pigment Yellow 150 (Y150) and 100 parts by mass of zirconia beads with a particle size of 2.0 mm are added and shaken for 1 hour with a paint shaker (manufactured by Asada Iron Works Co., Ltd.) for pre-disintegration. 200 parts of zirconia beads of 1 mm were used, and dispersion was carried out for 4 hours with a paint shaker as main pulverization to obtain a coloring material dispersion liquid G(1).
- the block copolymer 1 is salt-formed with phenylphosphonic acid to form a salt-type block copolymer 1 .
- Examples 25 to 34 Production of photosensitive colored resin compositions G-2 to G-11
- the type and / or mass ratio of the non-reactive resin was changed, and the formula (A-2) represented Photosensitive colored resin composition G-1 except that the ratio of the oxime ester photoinitiator was the same as in Example 24, and the mass ratio of the polyfunctional monomer was changed so that the pigment concentration was the same as in Example 24.
- photosensitive colored resin compositions G-2 to G-11 were obtained.
- Example 45 Production of photosensitive colored resin composition G-22
- 111 parts by mass of the colorant dispersion G (1) obtained above 10 parts by mass of the non-reactive resin 1 obtained in Synthesis Example 1, a polyfunctional monomer (trade name Aronix M-305, Toagosei Co., Ltd.
- Example 46 Production of photosensitive colored resin composition G-23)
- the polyfunctional epoxy compound was changed to a polyfunctional blocked isocyanate compound (trade name Duranate MF-K60B, manufactured by Asahi Kasei Corporation)
- photosensitive coloring was performed in the same manner as for the photosensitive colored resin composition G-22.
- a resin composition G-23 was obtained.
- Example 47 Production of photosensitive colored resin composition B-1) (1) Production of Colorant Dispersion B (1) In a 225 mL mayonnaise bottle, 48.1 parts by mass of PGMEA, 10 parts by mass of the alkali-soluble resin A solution of Preparation Example 1 (solid content: 40% by mass), and the block of Preparation Example 12 6.8 parts by mass of a PGMEA solution of copolymer 1 (solid content: 35% by mass) was added and stirred. 0.3 parts by mass of phenylphosphonic acid (trade name: PPA, manufactured by Nissan Chemical Industries, Ltd.) was added thereto, and the mixture was stirred at room temperature for 30 minutes. C.I. I.
- Pigment Blue 15:6 (B15:6) was added at 7.1 parts by mass, and C.I. I. 1.8 parts by mass of Pigment Violet 23 (V23) and 100 parts by mass of zirconia beads with a particle size of 2.0 mm were added, and the mixture was shaken for 1 hour with a paint shaker (manufactured by Asada Iron Works Co., Ltd.) for preliminary crushing. 200 parts of zirconia beads of 1 mm were used, and dispersion was carried out for 4 hours with a paint shaker as main pulverization to obtain a coloring material dispersion liquid B(1).
- the block copolymer 1 is salt-formed with phenylphosphonic acid to form a salt-type block copolymer 1 .
- Example 48 to 57 Production of photosensitive colored resin compositions B-2 to B-11
- the type and / or mass ratio of the non-reactive resin was changed, and represented by the formula (A-2)
- the ratio of the oxime ester photoinitiator remains the same as in Example 47, except that the mass ratio of the polyfunctional monomer is changed so that the pigment concentration is the same as in Example 47.
- Photosensitive colored resin composition B-1 In the same manner as above, photosensitive colored resin compositions B-2 to B-11 were obtained.
- Example 68 Production of photosensitive colored resin composition B-22
- a polyfunctional monomer trade name Aronix M-305, Toagosei Co., Ltd.
- Example 69 Production of photosensitive colored resin composition B-273
- the polyfunctional epoxy compound was changed to a polyfunctional blocked isocyanate compound (trade name Duranate MF-K60B, manufactured by Asahi Kasei Corporation).
- a colorant resin composition B-23 was obtained.
- Comparative Examples 1 to 6 Production of Comparative Photosensitive Colored Resin Compositions CR-1 to CR-6)
- Example 1 As shown in Table 5, except that no non-reactive resin was used or any of the comparative non-reactive resins c1 to c5 was used instead of non-reactive resin 1
- Comparative photosensitive colored resin compositions CR-1 to CR-6 were obtained in the same manner as the colored resin composition R-1.
- the photosensitive colored resin composition obtained in each example and each comparative example was coated on a glass substrate (manufactured by NH Techno Glass Co., Ltd., "NA35") using a spin coater to form a cured coating film having a thickness. After coating to a thickness of 3.0 ⁇ m, it was dried at 80° C. for 3 minutes using a hot plate to form a coating film on the substrate. This coating film is exposed to ultraviolet rays of 50 mJ/cm 2 using an ultra-high pressure mercury lamp through a photomask (chromium mask) having a pattern with an opening size of 2 ⁇ m to 100 ⁇ m for forming independent fine lines. A postcoat was formed.
- a photomask chromium mask
- ⁇ Cross-sectional shape evaluation of fine line pattern colored layer The cross-sectional shape in the thickness direction of the resulting colored layer in the form of an independent fine line pattern was observed with a scanning electron microscope (manufactured by Shimadzu Corporation, super scan model 220, magnification of 10,000 times). The taper angle ( ⁇ 1) of the cross-sectional shape (see FIG. 5) was evaluated.
- Examples 1 to 69 which are photosensitive colored resin compositions according to the present invention
- the alkali-soluble resin was combined with a specific non-reactive resin, so that the generation of development residue was suppressed even in low-temperature heat treatment, and It was shown that a colored layer with a good pattern shape can be formed.
- the non-reactive resin the use of a non-reactive resin in which the content of structural units derived from methyl methacrylate is 90% by mass to 99% by mass in all structural units is shown to improve the cross-sectional shape. was done.
- the addition of a polyfunctional epoxy resin or a polyfunctional isocyanate compound among others improves the solvent resistance.
- Comparative Example 2 in which a non-reactive resin having an acid value and a weight average molecular weight in the same range as the non-reactive resin of the present invention but using a butyl methacrylate monomer instead of a methyl methacrylate monomer was combined with an alkali-soluble resin.
- the photosensitive colored resin compositions Nos. 8 and 14 the cross-sectional shape of the colored layer was shown to be an undercut shape.
- Comparative Examples 3, 9 and 15 a non-reactive resin having a structural unit and an acid value in the same range as the non-reactive resin of the present invention but having a weight-average molecular weight larger than the specific value of the present invention was combined with an alkali-soluble resin. It has been shown that the photosensitive colored resin composition leaves a development residue in the colored layer formation area. Further, in Comparative Examples 4, 10 and 16, a non-reactive resin having a constitutional unit and an acid value in the same range as the non-reactive resin of the present invention but having a weight average molecular weight lower than the specific value of the present invention was combined with an alkali-soluble resin.
- the cross-sectional shape of the colored layer of the photosensitive colored resin composition becomes an undercut shape.
- the weight average molecular weight is in the same range as the non-reactive resin of the present invention, but the content of structural units derived from methyl methacrylate is 100 mol% of all structural units, and the acid value is 0 mgKOH/g.
- the photosensitive colored resin compositions of Comparative Examples 5, 11 and 17 in which the was combined with an alkali-soluble resin were shown to produce development residues in the colored layer formation portion.
Landscapes
- Physics & Mathematics (AREA)
- General Physics & Mathematics (AREA)
- Spectroscopy & Molecular Physics (AREA)
- Engineering & Computer Science (AREA)
- Optics & Photonics (AREA)
- Manufacturing & Machinery (AREA)
- Architecture (AREA)
- Structural Engineering (AREA)
- Chemical & Material Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Theoretical Computer Science (AREA)
- Optical Filters (AREA)
- Materials For Photolithography (AREA)
- Electroluminescent Light Sources (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2023530346A JPWO2022270358A1 (cg-RX-API-DMAC7.html) | 2021-06-25 | 2022-06-14 | |
| KR1020247001782A KR20240026179A (ko) | 2021-06-25 | 2022-06-14 | 감광성 착색 수지 조성물, 경화물, 컬러 필터, 표시 장치, 및 유기 발광 소자와 외광 반사 방지막의 적층체의 제조 방법 |
| CN202280040331.0A CN117480452A (zh) | 2021-06-25 | 2022-06-14 | 感光性着色树脂组合物、固化物、滤色器、显示设备、和有机发光元件与防外光反射膜的层叠体的制造方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021105552 | 2021-06-25 | ||
| JP2021-105552 | 2021-06-25 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022270358A1 true WO2022270358A1 (ja) | 2022-12-29 |
Family
ID=84544886
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2022/023797 Ceased WO2022270358A1 (ja) | 2021-06-25 | 2022-06-14 | 感光性着色樹脂組成物、硬化物、カラーフィルタ、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 |
Country Status (4)
| Country | Link |
|---|---|
| JP (1) | JPWO2022270358A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20240026179A (cg-RX-API-DMAC7.html) |
| CN (1) | CN117480452A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2022270358A1 (cg-RX-API-DMAC7.html) |
Cited By (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP7407330B1 (ja) | 2023-03-06 | 2023-12-28 | 東洋インキScホールディングス株式会社 | 感光性組成物、膜、光学フィルタ、固体撮像素子、画像表示装置、及び赤外線センサ |
| WO2025033443A1 (ja) * | 2023-08-07 | 2025-02-13 | 三菱ケミカル株式会社 | 着色剤分散液、着色樹脂組成物、硬化物、カラーフィルタ、液晶表示装置及び有機el表示装置 |
| KR20250093154A (ko) | 2023-12-15 | 2025-06-24 | 아티엔스 가부시키가이샤 | 경화성 조성물, 그것을 이용한 막, 광학 필터, 고체 촬상 소자, 화상 표시 장치, 및 적외선 센서 |
| WO2025142373A1 (ja) * | 2023-12-26 | 2025-07-03 | 株式会社Dnpファインケミカル | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 |
| WO2026070583A1 (ja) * | 2024-09-27 | 2026-04-02 | 株式会社Dnpファインケミカル | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 |
Citations (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2010015025A (ja) * | 2008-07-04 | 2010-01-21 | Adeka Corp | 特定の光重合開始剤を含有する感光性組成物 |
| WO2017030005A1 (ja) * | 2015-08-17 | 2017-02-23 | 株式会社Adeka | 組成物 |
| JP2019038985A (ja) * | 2017-08-25 | 2019-03-14 | 東洋インキScホールディングス株式会社 | アゾ顔料、カラーフィルタ用着色剤、着組成物およびカラーフィルタ |
Family Cites Families (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| KR102335614B1 (ko) | 2018-03-21 | 2021-12-03 | 동우 화인켐 주식회사 | 착색 감광성 수지 조성물, 이를 포함하는 컬러필터 및 화상표시장치 |
-
2022
- 2022-06-14 JP JP2023530346A patent/JPWO2022270358A1/ja active Pending
- 2022-06-14 WO PCT/JP2022/023797 patent/WO2022270358A1/ja not_active Ceased
- 2022-06-14 KR KR1020247001782A patent/KR20240026179A/ko active Pending
- 2022-06-14 CN CN202280040331.0A patent/CN117480452A/zh active Pending
Patent Citations (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2010015025A (ja) * | 2008-07-04 | 2010-01-21 | Adeka Corp | 特定の光重合開始剤を含有する感光性組成物 |
| WO2017030005A1 (ja) * | 2015-08-17 | 2017-02-23 | 株式会社Adeka | 組成物 |
| JP2019038985A (ja) * | 2017-08-25 | 2019-03-14 | 東洋インキScホールディングス株式会社 | アゾ顔料、カラーフィルタ用着色剤、着組成物およびカラーフィルタ |
Cited By (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP7407330B1 (ja) | 2023-03-06 | 2023-12-28 | 東洋インキScホールディングス株式会社 | 感光性組成物、膜、光学フィルタ、固体撮像素子、画像表示装置、及び赤外線センサ |
| JP2024125989A (ja) * | 2023-03-06 | 2024-09-19 | artience株式会社 | 感光性組成物、膜、光学フィルタ、固体撮像素子、画像表示装置、及び赤外線センサ |
| WO2025033443A1 (ja) * | 2023-08-07 | 2025-02-13 | 三菱ケミカル株式会社 | 着色剤分散液、着色樹脂組成物、硬化物、カラーフィルタ、液晶表示装置及び有機el表示装置 |
| KR20250093154A (ko) | 2023-12-15 | 2025-06-24 | 아티엔스 가부시키가이샤 | 경화성 조성물, 그것을 이용한 막, 광학 필터, 고체 촬상 소자, 화상 표시 장치, 및 적외선 센서 |
| JP2025095551A (ja) * | 2023-12-15 | 2025-06-26 | artience株式会社 | 硬化性組成物、それを用いた膜、光学フィルタ、固体撮像素子、画像表示装置、及び赤外線センサ |
| JP7704188B2 (ja) | 2023-12-15 | 2025-07-08 | artience株式会社 | 硬化性組成物、それを用いた膜、光学フィルタ、固体撮像素子、画像表示装置、及び赤外線センサ |
| WO2025142373A1 (ja) * | 2023-12-26 | 2025-07-03 | 株式会社Dnpファインケミカル | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 |
| WO2026070583A1 (ja) * | 2024-09-27 | 2026-04-02 | 株式会社Dnpファインケミカル | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| JPWO2022270358A1 (cg-RX-API-DMAC7.html) | 2022-12-29 |
| CN117480452A (zh) | 2024-01-30 |
| KR20240026179A (ko) | 2024-02-27 |
| TW202311316A (zh) | 2023-03-16 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP5929496B2 (ja) | 感放射線性樹脂組成物、表示素子用硬化膜、表示素子用硬化膜の形成方法及び表示素子 | |
| KR20240026179A (ko) | 감광성 착색 수지 조성물, 경화물, 컬러 필터, 표시 장치, 및 유기 발광 소자와 외광 반사 방지막의 적층체의 제조 방법 | |
| JP5668539B2 (ja) | カラーフィルタ用着色組成物、カラーフィルタ及びカラー液晶表示素子 | |
| KR20110019979A (ko) | 착색 감광성 수지 조성물, 이를 이용하여 제조된 컬러필터 및 액정표시장치 | |
| TWI709818B (zh) | 具有間隔件功能的遮光膜用的感光性樹脂組成物、遮光膜、液晶顯示裝置、具有間隔件功能的遮光膜用的感光性樹脂組成物的製造方法、遮光膜的製造方法以及液晶顯示裝置的製造方法 | |
| JP2012083753A (ja) | 着色感光性樹脂組成物、カラーフィルター及び液晶表示装置 | |
| WO2024171742A1 (ja) | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 | |
| TWI491984B (zh) | 用於彩色濾光片的光敏樹脂組合物及使用其的彩色濾光片 | |
| WO2023140087A1 (ja) | 感光性着色樹脂組成物、硬化物、カラーフィルタ、表示装置 | |
| JP2003231752A (ja) | 感光性ポリイミド前駆体、感光性樹脂組成物、カラーフィルター、液晶駆動側基板、及び、液晶パネル | |
| JP2014005466A (ja) | アルカリ可溶性樹脂、それを含む感光性樹脂組成物およびそれを用いたカラーフィルタ | |
| KR102909589B1 (ko) | 감광성 착색 수지 조성물, 경화물, 컬러 필터, 표시 장치 | |
| KR102924059B1 (ko) | 광경화성 착색 수지 조성물, 경화물, 컬러 필터, 표시 장치 | |
| JP2016126324A (ja) | 着色感光性樹脂組成物 | |
| WO2025142373A1 (ja) | 感光性着色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 | |
| JP4251442B2 (ja) | 感光性パターン形成用硬化性樹脂組成物、液晶パネル用基板、及び、液晶パネル | |
| JP7263031B2 (ja) | 色材分散液、分散補助樹脂、感光性着色樹脂組成物及びその硬化物、カラーフィルタ、表示装置 | |
| JP6450057B1 (ja) | 感光性着色樹脂組成物及びその硬化物、カラーフィルタ、並びに表示装置 | |
| WO2022176831A1 (ja) | 感光性緑色樹脂組成物、硬化物、カラーフィルタ、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 | |
| TWI914492B (zh) | 感光性著色樹脂組合物、硬化物、彩色濾光片、及顯示裝置 | |
| JP2009025820A (ja) | 着色感光性樹脂組成物及びその着色感光性樹脂組成物を用いて得られるカラーフィルタ並びにそのカラーフィルタを備える液晶表示装置 | |
| JP7627547B2 (ja) | 色材分散液、分散剤、着色硬化性組成物、カラーフィルタ、表示装置 | |
| JP7822361B2 (ja) | 光硬化性緑色樹脂組成物、表示装置、及び有機発光素子と外光反射防止膜の積層体の製造方法 | |
| JP7731799B2 (ja) | 色材分散液、分散剤、感光性着色樹脂組成物、硬化物、カラーフィルタ、表示装置 | |
| TW200911523A (en) | Dry film, micro-lens and manufacturing method thereof as well as liquid crystal display element with micro-lens |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22828275 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023530346 Country of ref document: JP |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280040331.0 Country of ref document: CN |
|
| ENP | Entry into the national phase |
Ref document number: 20247001782 Country of ref document: KR Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1020247001782 Country of ref document: KR |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |