WO2022237966A1 - Network of metal fibers and method of assembling a fiber network - Google Patents

Network of metal fibers and method of assembling a fiber network Download PDF

Info

Publication number
WO2022237966A1
WO2022237966A1 PCT/EP2021/062435 EP2021062435W WO2022237966A1 WO 2022237966 A1 WO2022237966 A1 WO 2022237966A1 EP 2021062435 W EP2021062435 W EP 2021062435W WO 2022237966 A1 WO2022237966 A1 WO 2022237966A1
Authority
WO
WIPO (PCT)
Prior art keywords
fibers
metal fibers
assembling
network
less
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/EP2021/062435
Other languages
English (en)
French (fr)
Inventor
Maximilian HACKNER
Joachim Spatz
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Max-Planck-Gesellschaft zur Förderung der Wissenschaften eV
Original Assignee
Max-Planck-Gesellschaft zur Förderung der Wissenschaften eV
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Max-Planck-Gesellschaft zur Förderung der Wissenschaften eV filed Critical Max-Planck-Gesellschaft zur Förderung der Wissenschaften eV
Priority to PCT/EP2021/062435 priority Critical patent/WO2022237966A1/en
Priority to CN202280026643.6A priority patent/CN117157438B/zh
Priority to ES22728541T priority patent/ES3010516T3/es
Priority to JP2023554284A priority patent/JP2024521238A/ja
Priority to KR1020237036354A priority patent/KR20240006512A/ko
Priority to PCT/EP2022/062655 priority patent/WO2022238413A1/en
Priority to EP22728541.8A priority patent/EP4281608B1/en
Priority to US18/289,128 priority patent/US20240367228A1/en
Publication of WO2022237966A1 publication Critical patent/WO2022237966A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • D—TEXTILES; PAPER
    • D04—BRAIDING; LACE-MAKING; KNITTING; TRIMMINGS; NON-WOVEN FABRICS
    • D04H—MAKING TEXTILE FABRICS, e.g. FROM FIBRES OR FILAMENTARY MATERIAL; FABRICS MADE BY SUCH PROCESSES OR APPARATUS, e.g. FELTS, NON-WOVEN FABRICS; COTTON-WOOL; WADDING ; NON-WOVEN FABRICS FROM STAPLE FIBRES, FILAMENTS OR YARNS, BONDED WITH AT LEAST ONE WEB-LIKE MATERIAL DURING THEIR CONSOLIDATION
    • D04H1/00—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres
    • D04H1/40—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties
    • D04H1/42—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties characterised by the use of certain kinds of fibres insofar as this use has no preponderant influence on the consolidation of the fleece
    • D04H1/4209—Inorganic fibres
    • D04H1/4234—Metal fibres
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D39/00—Filtering material for liquid or gaseous fluids
    • B01D39/14—Other self-supporting filtering material ; Other filtering material
    • B01D39/20—Other self-supporting filtering material ; Other filtering material of inorganic material, e.g. asbestos paper, metallic filtering material of non-woven wires
    • B01D39/2027—Metallic material
    • B01D39/2041—Metallic material the material being filamentary or fibrous
    • B01D39/2044—Metallic material the material being filamentary or fibrous sintered or bonded by inorganic agents
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
    • B22F1/05—Metallic powder characterised by the size or surface area of the particles
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
    • B22F1/06—Metallic powder characterised by the shape of the particles
    • B22F1/062—Fibrous particles
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
    • B22F1/08—Metallic powder characterised by particles having an amorphous microstructure
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/002—Manufacture of articles essentially made from metallic fibres
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B22F3/1017—Multiple heating or additional steps
    • B22F3/1028—Controlled cooling
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B22F3/11—Making porous workpieces or articles
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B22F3/11—Making porous workpieces or articles
    • B22F3/1103—Making porous workpieces or articles with particular physical characteristics
    • D—TEXTILES; PAPER
    • D04—BRAIDING; LACE-MAKING; KNITTING; TRIMMINGS; NON-WOVEN FABRICS
    • D04H—MAKING TEXTILE FABRICS, e.g. FROM FIBRES OR FILAMENTARY MATERIAL; FABRICS MADE BY SUCH PROCESSES OR APPARATUS, e.g. FELTS, NON-WOVEN FABRICS; COTTON-WOOL; WADDING ; NON-WOVEN FABRICS FROM STAPLE FIBRES, FILAMENTS OR YARNS, BONDED WITH AT LEAST ONE WEB-LIKE MATERIAL DURING THEIR CONSOLIDATION
    • D04H1/00—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres
    • D04H1/40—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties
    • D04H1/54—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties by welding together the fibres, e.g. by partially melting or dissolving
    • D—TEXTILES; PAPER
    • D04—BRAIDING; LACE-MAKING; KNITTING; TRIMMINGS; NON-WOVEN FABRICS
    • D04H—MAKING TEXTILE FABRICS, e.g. FROM FIBRES OR FILAMENTARY MATERIAL; FABRICS MADE BY SUCH PROCESSES OR APPARATUS, e.g. FELTS, NON-WOVEN FABRICS; COTTON-WOOL; WADDING ; NON-WOVEN FABRICS FROM STAPLE FIBRES, FILAMENTS OR YARNS, BONDED WITH AT LEAST ONE WEB-LIKE MATERIAL DURING THEIR CONSOLIDATION
    • D04H1/00—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres
    • D04H1/40—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties
    • D04H1/54—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties by welding together the fibres, e.g. by partially melting or dissolving
    • D04H1/556—Non-woven fabrics formed wholly or mainly of staple fibres or like relatively short fibres from fleeces or layers composed of fibres without existing or potential cohesive properties by welding together the fibres, e.g. by partially melting or dissolving by infrared heating
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
    • H01M4/134—Electrodes based on metals, Si or alloys
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/06—Filter cloth, e.g. knitted, woven non-woven; self-supported material
    • B01D2239/0604—Arrangement of the fibres in the filtering material
    • B01D2239/0618—Non-woven
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/10—Filtering material manufacturing
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/12—Special parameters characterising the filtering material
    • B01D2239/1208—Porosity
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/12—Special parameters characterising the filtering material
    • B01D2239/1225—Fibre length
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/12—Special parameters characterising the filtering material
    • B01D2239/1233—Fibre diameter
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D2239/00—Aspects relating to filtering material for liquid or gaseous fluids
    • B01D2239/12—Special parameters characterising the filtering material
    • B01D2239/1241—Particle diameter
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01D—SEPARATION
    • B01D39/00—Filtering material for liquid or gaseous fluids
    • B01D39/10—Filter screens essentially made of metal
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F2304/00—Physical aspects of the powder
    • B22F2304/10—Micron size particles, i.e. above 1 micrometer up to 500 micrometer
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F2998/00—Supplementary information concerning processes or compositions relating to powder metallurgy
    • B22F2998/10—Processes characterised by the sequence of their steps
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/64—Carriers or collectors
    • H01M4/66—Selection of materials
    • H01M4/661—Metal or alloys, e.g. alloy coatings
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/64—Carriers or collectors
    • H01M4/70—Carriers or collectors characterised by shape or form
    • H01M4/80—Porous plates, e.g. sintered carriers
    • H01M4/801—Sintered carriers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/64—Carriers or collectors
    • H01M4/70—Carriers or collectors characterised by shape or form
    • H01M4/80—Porous plates, e.g. sintered carriers
    • H01M4/806—Nonwoven fibrous fabric containing only fibres

Definitions

  • the invention relates to a method of assembling a fiber network comprising a plu rality of metal fibers as well as to a network of metal fibers.
  • Networks of fibers are nowadays used for a great variety of applications ranging for example from filters to batteries.
  • filters are usually based on metal fibers comprising a circu lar cross section (e. g. oil filters) or on carbon-based foams (e. g. HEPA filters).
  • Filters made out of metal fibers with circular cross sections are characterized in that such fibers comprise a high mechanical stability while comprising small surface to volume ratios.
  • filters usually comprise a rather high weight since a great amount of fibers is needed.
  • Filters made out of carbon foams are mostly rather fragile while being light weighted and having a rather large inner surface area. Furthermore, it is noted that the filtration capacity of such con ventionally known filters is not ideal.
  • networks of metal fibers can also improve the perfor mance of secondary batteries when being used as secondary electrodes.
  • Such networks of metal fibers can also contribute to the performance in catalytic materi als in electrochemical applications such as in fuel cells and hydrolysis, or as com ponent in electromagnetic shielding materials, as filters, in polymer composites or as tissue material and tissue hybrid material which may also include as additives, e.g. cotton, silk or wool.
  • a plurality of fi bers is provided in a hot press and subjected to a high pressure. Then the plurality of fibers is placed in a furnace and slowly heated up to a temperature close to the melting temperature of the fibers while the plurality of fibers still being subjected to said pressure. The high temperature is maintained until the fibers connect to one another. Afterwards, the fabricated network is slowly cooled down.
  • sintering Such processes usually take up to one hour or more depending on the capacity of the oven used. It was now recognized that conventional sintering allows fibers to undergo relaxation be fore reaching temperatures high enough to connect the fibers to one another. These relaxation processes release stored energy from the fibers. As an example, fibers obtained by rapid cooling techniques, e.g. melt spinning, can have substan tial amounts of stored energy.
  • the driving force for the above described process is the reduction of the surface of the fibers and the associated reduction in their free energy AG.
  • the free energy AG can be divided into a surface component AGs, a volume component AGv and a grain boundary component AG B . This relationship is described in equation (1).
  • the volume part AGv clearly outweighs the grain boundary part AG B , which leads to a negative change in the total free energy of the system (AG ⁇ 0) and the process takes place voluntarily as soon as a certain energy threshold (activation energy) is exceeded.
  • activation energy energy
  • reduction of AG is as sociated also with a rounding of the fibers, i.e. the fiber diameter transitions into a round shape, herein also referred to as rounding.
  • the energy threshold to be exceeded here is the activation energy EA of the diffu sion (equation (2)).
  • Do is the temperature-dependent diffusion constant
  • k the Boltzmann constant
  • T the absolute temperature
  • D the temperature-depend ent diffusion constant.
  • the tempera ture is not only responsible for fulfilling the activation energy EA, but also the speed-determining factor.
  • thermodynamic goal is to achieve the largest possible volume with the smallest possible surface.
  • the perfect ratio here is achieved with a perfect sphere.
  • the present invention provides a method of assembling a fiber net work, comprising a plurality of metal fibers, wherein the method comprises the fol lowing steps: providing a loose network out of the plurality of metal fibers at an assem bling site; fixing the plurality of metal fibers to one another by forming contact points between the single metal fibers by:
  • cooling the plurality of fibers at a cooling rate higher than 20 K/min, prefera bly higher than 50 K/min, preferably higher than 100 K/min, in particular to a temperature below 60% of their melting point.
  • fibers which are subjected to heat tend to rearrange at an atomic level such that the largest possible volume with the smallest possible sur face is achieved.
  • the “most perfect” state, as seen from the fiber’s point of view, is a perfect sphere.
  • the fibers start to rear range at their atomic level, because of the heating step, to reach a more prefera ble energy level by, for example, crystallizing or by reducing defects in the crystal lattice of the fiber.
  • the fibers may even change their shape by transforming their cross section form a flat or elliptic cross section into a circular cross section, i.e. rounding of the fibers’ cross sectional shape occurs.
  • the fibers show sections with reduced diameters, herein referred to as constrictions. These constrictions develop further until the fibers are inter rupted. Ultimately, the fibers transform into a plurality of droplets, i.e. they reach a spherical form.
  • the method of the present invention utilizes the kinetics of said rearrangement process.
  • the rearrangement only takes place, when the fibers have sufficient time to do so.
  • By increasing the heating rate as well as the cooling rate and by keeping the fixation temperature equal to or less than 30 minutes it can be ensured that the metal fibers create contact points where they connect with one another.
  • said rearrangement processes are reduced drastically and especially the shape changing effect, i.e. the rounding and the formation of constrictions and in terruptions, can be avoided. Therefore, in the method of the present invention the heating rates as well as the cooling rates are kept well above 20 K/min, preferably higher than 50 K/min, preferably higher than 100 K/min.
  • the cooling rate is not as crucial anymore and may thus also be lowered if necessary.
  • Commonly known sintering processes take place at heating/cooling rates of about 10 to 20 K/min, thereby taking much longer to heat/cool the fibers (up to hours).
  • the heating rate is too low, relaxation processes may occur in the loose network of metal fibers before reaching the fixation temperature, reducing the surface component AGs and the grain boundary component AGB of the free energy.
  • step A when a low heating rate is applied in step A, the fixation time of 30 minutes or less in step B might be insufficient for fixing the fibers to one another, since the fixation cannot benefit to the same extend from surface component AGs and grain bound ary component AGB as when applying the higher heating rates in step A. Requiring more time for reaching the fixation temperature and/or keeping the fibers at a longer time at the fixation temperature results in the fibers being transformed into a thermodynamically more favored state, i.e. the cross section of the fibers may change towards round.
  • the loose network of fibers can be assembled to a network of fixed fibers with minimal (unwanted) effects on their atomic level.
  • the fibers’ cross sectional shape and length can be maintained.
  • the fibers are in a thermodynamically more stable state when reaching the fixation temperatures.
  • higher fixation temperatures and higher fixation times are required, driving a change of the fibers’ cross sections, diame ters and/or lengths.
  • the temperature applied i.e. the fixation temperature
  • the crystallization temperature can, for example, be determined by differential scanning calorimetry (DSC) measurement for the metal fibers in question. DSC measurement can be performed using the following conditions: Starting tempera ture 30 °C with a heating rate of 10 K min-1 until 1200 °C, continued with a cooling rate of 10 K min-1 until room temperature.
  • DSC measurements may be performed in an argon atmosphere with a constant argon flow of 100 ml min-1 and a zirco- nium-oxygen-trap system for a complete oxygen free atmosphere (STA 449 F3 Ju piter, Netzsch Bj. 2017).
  • % of the melting temperature refers to the melting temperature in °C, as determined by, for example, differential scanning calorimetry (DSC) measurements. Accordingly, if the melting tempera ture is 1000 °C, in the context of the description of the invention 20% of the melt ing temperature is 200 °C, 50% of the melting temperature is 500 °C and 95% of the melting temperature is 950 °C.
  • a network can be assembled which is flexible and can be deformed repeatedly with out causing degradation of the network, i.e. without separating single metal fibers out of the network of metal fibers due to deformation.
  • the metal fibers are fixed to one another, so that the metal fibers contact each other, i.e. the point of contact is not movable relative to the metal fibers as it is the case for example in a nonwoven agglomeration of entangled metal fibers, such as a metal felt.
  • the network of metal fibers according to the invention is mechanically stable yet flexible. Mechanically stable in this context means that the network of metal fibers is not a loose agglomeration of metal fibers, i.e.
  • the network does not disintegrate into isolated metal fibers as soon as a small force acts on the network.
  • a network of metal fibers can be flexibly deformed without breaking. It is possible that the network of metal fibers recovers its form after deformation. Flowever, if the network of metal fibers is folded, it is also possible to reshape it permanently.
  • the contact points are distributed throughout the whole assembled network, so that throughout the 3-dimensional structure of the network of metal fibers contact points are pre sent. Accordingly, the contact points are not only provided in a certain area of the network of metal fibers such as in the center or in the circumference of the net work. It could be possible that the points of contact are evenly distributed through out the network.
  • the density of contact points has a gradient throughout the network, i.e. that the network has areas with a higher den sity of contact points and areas with a lower density of contact. It is also possible to have ordered or random spatial distributions of contact points.
  • each of the metal fibers can have at least two contact points with other metal fibers, more preferably at least three contact points, even more preferably at least four contact points.
  • the method before fixing the plurality of metal fibers to one an other the method further comprises a step of subjecting the plurality of metal fibers to a predetermined pressure, which is in particular less than 1 MPa, especially less than 500 kPa.
  • a predetermined pressure which is in particular less than 1 MPa, especially less than 500 kPa.
  • a protective gas at said assembling site such as argon, nitrogen, Ar-W5 (5 vol.-% H2 in Ar), Ar-W2 (2 vol.-% H2 in Ar), a forming gas (5 vol.-% H2 in N2) or other noble gases in order to avoid oxidation of the fi bers during the assembling process.
  • a protective gas such as argon, nitrogen, Ar-W5 (5 vol.-% H2 in Ar), Ar-W2 (2 vol.-% H2 in Ar), a forming gas (5 vol.-% H2 in N2) or other noble gases in order to avoid oxidation of the fi bers during the assembling process.
  • the method according to the inven tion can also be carried out in vacuum.
  • the precise conditions at the assem bling site may be chosen, for example, depending on the materials used for the fi bers. For instance, some materials such as iron and/or some steels cannot be used together with nitrogen since they tend to nitriding. Therefore, for such materi als another protective gas may
  • the step of heating the fibers is carried out by a suitable heating device.
  • a suitable heating device Preferred examples for such heating de vices are induction furnaces, infrared furnaces, high temperature ceramic heating elements and/or zone furnaces such as, for example, conveyor furnaces.
  • Such heating devices can ensure a fast heating, i.e. high heating rates, as well as fast cooling, i.e. high cooling rates, such that the plurality of fibers can be connected to one another without having the fibers loose too much energy due to rearrange ment and relaxation processes or anything alike before reaching the fixation tem perature.
  • the heating device may suitably be a continuous furnace or a batch fur nace.
  • the fixation temperature is determined in-situ by electron micros copy. This can be done, for example, by placing fibers in an in-situ SEM (scanning electron microscope) heating stage. The fibers need a good thermal connection to the heating stage due to the nearly non-existing heat transfer in a high vacuum.
  • SEM scanning electron microscope
  • heat stabile graphite papers can be used.
  • one sheet may be used as support between the fibers and the heating stage and another one with a hole in the middle may be used to view the fibers.
  • These fiber sandwiches may then be transferred to the heating stage and pressed down.
  • the heating stage may be heated to a temperature which is close, but still lower than the melting temperature of the fibers.
  • the fiber cross-section may be observed with the SEM until the fibers start to connect to one another.
  • the fixa tion temperature may be determined.
  • the fiber sandwich may be heated at a heating rate, as mentioned above, to said determined fixation temperature.
  • Said fixation temperature may then be held for a fixation time until the wanted degree of connection and therefore the wanted strength of connection is reached.
  • the method steps A to C according to the invention may be carried out in order to check whether the deter mined fixation temperature is correct.
  • Fixation temperature and time depends on the material of the fibers, the dimension of the fibers, i.e. width and thickness, and the amount of stored energy in the fi bers. For example, for fine fibers of a given material having a low thickness and width rounding processes tend to occur faster compared to less fine fibers of the same material. Determining the fixation temperatures and times for a specific type of fiber is possible using either above mentioned in-situ by electron microscopy or by using trial and error tests. Trial and error tests can be carried out using the ac tual equipment for producing the network of metal fibers, i.e. under the actual man ufacturing conditions.
  • the fixation temperature i.e. the temperature maintained in step B
  • the fixation temperature is selected in the range of 80 to 98%, in particular in the range of 90 to 98%, of the melting temperature of the metal fibers. Fixation temperatures in said range turned out suitable for most materials.
  • the precise fixation temperature may also depend on the fixation time. That is, the higher the fixation temperature, the shorter the fixation time may be and vice versa.
  • the cooling rate in step C is preferably maintained for a sufficient period for the metal fibers to cool below 60% of the melting temperature of the metal fibers.
  • Steps A, B and C are carried out in a combined period of time which is preferably less than 30 minutes, preferably less than 15 minutes, in particular less than 5 minutes, especially less than 1 minute. It has shown that the faster the method is performed the less negative side effects occur, such as for example release of en ergy, formation of fiber constrictions and/or interruptions and change of fiber cross- sectional shape. Also in this context, it is to be noted that the cooling of step C does not necessarily require a cooling until room temperature. Step C may be ter minated after cooling to a temperature of 60% of the melting temperature of the metal fibers.
  • steps A, B and C may take much longer compared to steps A and C.
  • steps A and C may take 1 minute while step B may take 30 seconds.
  • step A may be car ried out within 1 to 5 minutes, step B within 0.5 to 1 minute and step C within 10 minutes until the assembled network is cooled down to a temperature of about 60% of the melting temperature of the used fibers.
  • the further cooling of the asflectd network to room temperature may, for example, take another 1 to 2 hours.
  • the metal fibers comprise a length of 1.0 mm or more and/or a width of 100 pm or less and/or a thickness of 50 pm or less.
  • the metal fibers having such dimensions, it is possible to produce the network with metal fibers that are fixed to one another, without needing to heat the metal fibers for a time of more than 30 minutes to temperatures close to their melting point.
  • Conventional sintering techniques require temperatures close or even slightly above the melting temperature of the metal to be maintained for a relatively long period of time. This can result in melting or at least softening the material of the metal fibers to a certain degree, so that the metal fibers form a metal foil rather than a network, in particular when relatively high pressure is applied during sinter ing.
  • the network of metal fibers is not a metal foil, i.e. the structure of the metal fibers used for producing the network of metal fibers can still be recognized in the network of metal fibers. Accordingly, in a cross-sectional view of network of metal fibers, there are voids which are not part of the metal fibers but are in be tween the metal fibers of the network fibers.
  • the metal fibers be fore fixing them one to another, show an exothermic event when heated in a DSC measurement, wherein the exothermic event releases energy in an amount of 0.1 kJ/g or more, more preferably in an amount of 0.5 kJ/g or more, even more prefer ably in an amount of 1.0 kJ/g or more and most preferably in an amount of 1.5 kJ/g or more.
  • the absolute amounts depend very much on the used metal or metal al loy.
  • the extent of the exothermic event can be determined by comparing DSC measurements of the metal fibers before and after thermal equilibration. In other words, the metal fibers showing such an exothermic event are not in their thermo dynamic equilibrium at ambient temperatures.
  • the metal fibers can transit from a metastable to a thermodynamically more stable condition, e.g. by crystallization, recrystallization or other relaxation pro Being reducing defects in the lattice of metal atoms.
  • An exothermic event ob served for the metal fibers when being heated, e.g. during a DSC measurement, indicates that the metal fibers are not in their thermodynamic equilibrium, e.g. the metal fibers can be in an amorphous or nanocrystalline state containing defective energy and/or crystallization energy which is released during heating of the metal fibers due to occurrence of crystallization or recrystallization.
  • Such events can be recognized e.g. using a DSC measurement. It was found that networks of metal fi bers which show such an exothermic event have an improved strength after the metal fibers are fixed to one another.
  • the metal fibers comprise a non-round cross section, in particular a rectangular, quadratic, partial circular or an elliptical cross section with a large axis and a small axis.
  • Such cross-sections usually lead to fi bers which are not in their thermal equilibrium, i. e. in a metastable state, which, for some applications, may be beneficial.
  • the value of the small axis must be smaller than the value of the large axis.
  • the definition of "small” and "large” must simply be interchanged.
  • a ratio of the small axis to the large axis lies in the range of 1 to 0.05, preferably in the range of 0.7 to 0.1 , in particular in the range of 0.5 to 0.1.
  • the ratio between the lengths of the small and the large axis of an ellipse is higher the more the ellipse looks like a circle, for which the ratio would be 1. The smaller the value of the ratio is, the flatter is the ellipse.
  • the ratio of the small axis to the large axis is in particular less than 1.
  • the metal fibers may comprise a round cross-section.
  • a ratio of a “large” axis to a “small” axis would obviously be exactly 1.
  • Round cross-sections comprise an energetically more preferred state the cross- sections comprising an aspect ratio that is smaller than 1.
  • fibers with round cross-sections are energetically closer to their equilibrium state than fibers with cross-sections of other shapes.
  • the metal fibers are obtainable by subjecting a molten material of the metal fibers to a cooling rate of 10 2 K min -1 or higher, in particular by vertical or horizontal melt spinning.
  • a cooling rate of 10 2 K min -1 or higher in particular by vertical or horizontal melt spinning.
  • Such metal fibers produced by melt spinning can contain spatially confined domains in a high-energy state (i. e. in a metastable state), due to the fast cooling applied during the melt spinning process.
  • Fast cooling in this regard refers to a cooling rate of 10 2 K min -1 or higher, preferably of 10 4 K min -1 or higher, more preferably to a cooling rate of 10 5 K-min 1 or higher.
  • fibers obtained by melt spinning often comprise a rectangular or semi-ellipti cal cross section, which are preferred for certain application fields since they are far away from their equilibrium state.
  • melt spinners with which such fibers can be produced are for example known from the not yet published interna tional application PCT/EP2020/063026 and from published applications WO201 6/020493 A1 and WO2017/042155 A1, which are hereby incorporated by reference.
  • At least some of the metal fibers of the plurality of metal fibers are amorphous or at least some of the metal fibers of the plurality of metal fibers are nanocrystalline.
  • Nanocrystalline metal fibers contain crystalline domains. Upon heating to a temperature of about 20-60% of the melting tempera ture of the nanocrystalline metal fibers, these domains undergo recrystallization re sulting in an increase of the average size of crystalline domains compared to the average size of the initial crystalline domains in the nanocrystalline metal fibers before heating. It is also possible to mix non-equilibrated (e.g. nanocrystalline or amorphous fibers) with equilibrated (e.g. annealed) fibers.
  • the metal fibers are in electrical contact with one another. This can for example be preferable if the assembled networks are supposed to be used in electrochemical applications, such as batteries, fuel cells or anything alike.
  • the metal fibers are in direct electrical contact with one another such that the electrical conductivity can be enhanced to a maximum.
  • all of the metal fibers are sintered to other metal fibers, most preferable directly to other metal fibers, without the need of an additional binder, e.g. a polymeric binder. It is therefore further preferred that the metal fibers are fixed to one another without a polymeric binder, since such polymeric binders often have a poor electrical conductivity and high temperature performance.
  • the metal fibers contain at least one of copper, silver, gold, nickel, palladium, platinum, cobalt, iron, chromium, vanadium, titanium, alu minum, silicon, lithium, manganese, boron, combinations of the foregoing and al loys containing one or more of the foregoing, such as CuSn8, CuSi4, AISi1 , Ni, stainless steel, Cu, Al or vitrovac alloys.
  • Vitrovac alloys are Fe-based and Co based amorphous alloys. It may particularly be preferred if the metal fibers are made of copper or of aluminum or of a stainless steel alloy.
  • the filter can contain for ex ample metal fibers made of copper, one or more stainless steel alloys and/or alu minum. Networks being made out of metal fibers, wherein the metal fibers are of copper, aluminum, cobalt, stainless steel alloys containing copper, aluminum, sili con and/or cobalt, are particularly preferred.
  • a network of metal fibers comprising a plurality of metal fibers fixed one to another at contact points, and wherein the metal fibers either comprise a non-round cross section, for example a rectangular, quadratic, partial circular or an elliptical cross section with a large axis and a small axis, or wherein the metal fibers comprise a round cross section.
  • the fibers further comprise a width which is generally con stant along a length of the fiber such that a variation of the width of the fiber along its length is preferably less than 40%, more preferably less than 30% or even more preferably less than 20%.
  • the width of the fibers along their length changes by less than 20%, more preferably by less than 10%, even more preferably by less than 5% or most preferably by less than 1%.
  • the change of the fibers’ widths refers herein to a comparison of a fiber width before and after sintering the fibers to one another.
  • the fibers usually comprise random shapes such that it cannot be ensured that the width of a single fiber does not vary very much along its length. If a fiber, for example, would comprise large variations of its width, it could be possible that said fiber would tear apart at a section which com prises a smaller width, i.e. the fiber has a constriction which turns then into an in terruption. Fibers with a (nearly) constant width, on the other hand, have to ad vantage that the single fibers can connect to one another at any given point along their length without showing the risk of being interrupted during this process.
  • the metal fibers are substan tially constant in width, i.e. the width variation of the fiber along its length is prefer ably less than 40%, more preferably less than 30% or even more preferably less than 20%.
  • the width variation of the fiber along its length is prefer ably less than 40%, more preferably less than 30% or even more preferably less than 20%.
  • the fibers transform into metal droplets when heated too long.
  • the method according to the invention utilizes fast heating and cooling rate and a reduced fixation time.
  • the fibers are substantially free of such interruptions such that the length of the fibers is preserved.
  • shape changes of the fibers cross section can be avoided, i.e. there is a kinetic control over the fiber shape.
  • the method of the present invention provides high control about the fiber shape.
  • the plurality of fibers is sintered one to another, more pre ferred directly sintered to one another. This ensures that no further frame or any thing alike is needed in order to keep the fibers together. Furthermore, by directly sintering the metal fibers to one another, the points of connection are electrically conductive. This provides a relatively low internal resistance for the network of metal fibers.
  • a ratio of the small axis to the large axis lies in the range of 1 to 0.05, preferably in the range of 0.7 to 0.1 , in particular in the range of 0.5 to 0.1.
  • fibers with a flatter cross-section are energeti cally wise further away from their equilibrium state such that they store more en ergy compared to fibers which comprise, for example, a round cross-section.
  • the characteristics network may in fact be possible to choose the characteristics network according to the application of the network by using fibers with a higher or lower ratio between the lengths of the small and large axis as described above.
  • the mechanical stability as well as the weight of the network de creases
  • the mechanical stability as well as the weight of the network increases.
  • the network is an ordered or an unordered network.
  • Such an unordered network has, for example, a good electrical conductivity in every direction and anisotropic fluidic properties. Moreover, it is easier to produce an unordered network of metal fibers, compared to an order network of fibers. Nevertheless, in some applications it may be preferred that the fibers in the net work are combed in different directions to provide directionality of individual fibers. Accordingly, it may be preferred that in the network some or all of the fibers have an orientation, i.e. the lengths of the fibers are not oriented randomly but have a predominant orientation in one or more spatial direction. By having a predominant orientation of the metal fibers, the filter can have isotropic fluidic properties.
  • the network has open pores be tween the metal fibers of the plurality of metal fibers.
  • the porosity of the network is preferably up to 95 vol%. It is also preferable that the porosity of the network is more than 80 vol%. It is even more preferable when the porosity is in the range of 80 vol% to 95 vol%. It is possible to incorporate active materials into the open pores, such as active electrode materials or active catalyst materials. It is further preferable that in the network according to the invention at least some of the metal fibers of the plurality of metal fibers are at least partially coated.
  • the coating can for example be an active material, such as an electrode active material which in teracts with Li-ions in batteries or a catalytically active material which coverts CO to C02 or is active in hydrolysis. It is also possible to apply a coating onto the metal fibers which improves the fixation of the metal fibers to one another, and thereby increases the mechanical strength of the network.
  • the porosity can be de termined using a micro-computertomograph to reproduce the network structure and then evaluate the porosity using the bubble point method described below.
  • such active electrode materials for batteries are: for the an ode: Graphite, Silicon, Silicon-Carbide (SiC) and Tin-Oxide (SnO), Tin-Dioxide (Sn02) and Lithium-Titanoxide (LTO); and for the cathode: Lithium-Nickel-Manga- nese-Cobalt-Oxide (NMC), Lithium-Nickel-Cobalt-Aluminium-Oxide (NCA), Lith- ium-Cobalt-Oxide (LiCo02) and Lithium-Iron-Phosphate (LFP).
  • NMC Lithium-Nickel-Manga- nese-Cobalt-Oxide
  • NCA Lithium-Nickel-Cobalt-Aluminium-Oxide
  • NCA Lith- ium-Cobalt-Oxide
  • LiCo02 Lithium-Iron-Phosphate
  • the network may comprise an average mean pore size selected in the range of 0.1 to 100 pm, preferably in the range of 0.5 to 50 pm, in particular in the range of 1 to 10 pm.
  • the mean pore size can be determined using a micro-computertomo graph to reproduce the fiber structure and then evaluate the mean pore diameter using the bubble point method.
  • the bubble point method determines the largest ball diameter, which might fit between two fibers, which is considered the pore size. More in detail, a point is placed at the center between two fibers and the ra dius of the bubble, with the point as a center is increased, until contact to the sur face of both fibers is made. The diameter of the bubble corresponds to the pore size. If at any given parameter the bubble diameter only contacts one fiber, the center point is displaced into the direction of the fiber that the bubble did not con tact.
  • the metal fibers are fixed, in particular directly fixed, to one another at points of contact which are randomly distributed throughout the network of metal fibers.
  • the points of contact are not randomly distributed but are provided e.g. in a peripheral region of the network of metal fibers or that the metal fibers are ordered so that also the point of contacts are ordered.
  • the points of contact at which the metal fi bers are fixed to one another are localized in specific areas and not provided evenly over the complete network of metal fibers. With the points of contact at which the metal fibers are fixed to one another being present only in separated ar eas, it is possible that the fibers inbetween these areas have a high flexibility whilte at the same time the mechanical stability and good electrical conductivity is ensured.
  • the thickness of the network of the invention is not particularly limited. However, it can be preferred if the network has a thickness of 0.01 mm or more. It is more pre ferred that the thickness of the network is 0.03 mm or more, even more preferred 0.05 mm or more, even more preferred 0.07 mm or more and most preferred 0.1 mm or more. If the thickness of the network is less than 0.01 mm, there is a risk that the mechanical stability of the network is not sufficient.
  • the upper limit for the thickness of the network is not particularly limited. However, depending on the ap- plication, the upper limit may be 3.0 mm or less, or 2.5 mm or less. For battery ap plications, a preferred thickness of the network is in the range from 0.1 mm to 0.5 mm. A network with a thickness in this range is advantageous concerning the stacking and rolling of the active material coated network for producing batteries. Another preferred thickness range is in the range of greater than 0.5 mm to 5 mm, more preferably in the range of 1 to 3 mm.
  • a network of metal fibers is provided, wherein said network may for example be the network according to the invention, that is obtainable by the method according the invention.
  • Fig. 1 an exemplary scheme illustrating typical processes that may occur during sintering
  • Fig. 2 frames of a video showing sintering and relaxation of CuSi4;
  • Fig. 3 frames of a video showing sintering and relaxation of AlSi 1 ;
  • Fig. 4 micrographs of a conventionally sintered fiber network
  • Fig. 5 micrographs of sintered CuSi4 fibers having a flat shape
  • FIG. 6 micrographs of sintered AlSi 1 fibers having a flat shape.
  • Figure 1 shows the typical diffusion processes causing relaxation during a sinter ing process. The different arrows show the surface diffusion 1 , the lattice diffusion (from the surface) 2, the evaporation and condensation 3, the grain boundary diffu sion 4, the lattice diffusion (from the boundary region) 5 and the volume diffusion 6. While processes 1-3 lead to no shrinkage and only connect the fibers to one an other, processes 4-6 remove material from the border region and deposit it on the sintered necks. The reason for this, as it is already explained above, is the reduc tion of the surface of the fibers and the associated reduction in their free energy AG.
  • the border region of the metal fibers is thermally activated so that the fibers 10 sinter together but not the whole fiber 10 is rounded in order to maintain the fiber shape and dimension, which may be associ ated with an enlarged surface providing beneficial properties for many applica tions, e.g. electrochemical applications or filtering applications.
  • a loose network of fibers 10 is provided at the assembling site 12. Said fibers 10 are then fixed to one another by forming points of contact 14 between the single fibers 10. For creating said contact points 14, the method according to the invention provides three steps:
  • the plurality of fibers 10 is heated at a heating rate higher than 50 K/min, in particular higher than 100 K/min, especially higher than 200 K/min, prefera bly higher than 1000 K/min, to a fixation temperature selected in the range of 50 to 98% of their melting point temperature.
  • fixation temperature is kept for a fixation time selected in the range of 30 seconds to 30 minutes.
  • said plurality of fibers 10 is cooled at a cooling rate higher than 50 K/min, preferably higher than 100 K/min, in particular to a temperature be low 60% of their melting point
  • the fibers 10 can be subjected to a pressure to ensure that the single fiber 10 come into contact with each other.
  • Said pressure can be relatively low, i.e. in the range of 0.05 to 1 GPa and serves the formation of contacts between the unconnected metal fibers. It is not necessary to maintain the pressure when carrying out steps A, B and C, i.e. it is sufficient to compress the fibers briefly by applying said pressure only before but not during carrying out steps A, B and C. It is preferred to not apply an external pressure force during steps A, B and C. By avoiding external pressure force, the risk of transforming the metal fibers into a metal foil can be avoided, in particular when operating with fixation temperatures close to the melting temperature.
  • steps A, B and C are performed more quickly.
  • a maximum time for performing all three steps can be defined as less than 45 minutes, even in the range of about 15 minutes. It could already be shown that times below 5 minutes and even below 1 minute are possi ble with the method according to the invention. This lies well below the common times used for sintering which conventionally takes up to several hours.
  • steps A, B and C are per formed with a furnace or another heating device which is configured to provide high heating and cooling rates such as an induction furnace, infrared furnace, high temperature ceramic heating elements and/or zone furnaces such as, for example, conveyor furnaces (not shown in the drawings).
  • a furnace or another heating device which is configured to provide high heating and cooling rates such as an induction furnace, infrared furnace, high temperature ceramic heating elements and/or zone furnaces such as, for example, conveyor furnaces (not shown in the drawings).
  • the fibers 10 which are supposed to be connected to one another are heated up to a precise fixation temperature which lie in the range of 50 to 98%, in particular in the range of 80 to 98%, more particular in the range of 90 to 98%, of the melting temperature of said fibers 10.
  • the precise fixation temperature depends on the materials used for the fibers 10 (see also Tables 1 and 2 below). Choosing the right fixation temperature allows to connect the fibers 10 to one another without having them start to change their shape, i. .e. to round, because of the above described relaxation processes, or without having them start to melt.
  • the heating stage is heated to a temperature close to the melting tem perature.
  • the fiber cross-section is then observed with the SEM until the fibers start to connect with one another. This way, the fixation temperature is deter mined.
  • the above mentioned steps A to C are carried out until the wanted degree of connection and therefore the wanted strength of con nection is reached.
  • an amount of fibers is placed in a fast heating furnace.
  • the network can be pressed together or placed on a plate with a space holder and a cover plate. After removing the air/oxygen in the furnace and setting the test at mosphere, the furnace is heated to the possible, i. e.
  • the determined, fixation tem perature and held for a certain time which might be the fixation time.
  • the parameters must be adjusted. In this connection it is noted that three possible outcomes can be ex pected: 1) the fibers are not sintered, 2) the fibers are sintered but round or 3) the fibers are not sintered but round.
  • the fixation temperature and/or fixation time should be increased.
  • the fixation tem perature and/or the fixation time should be decreased and for the third outcome the heating rate should be increased and the fixation temperature and/or the fixa tion time decreased.
  • a protective gas such as for example ar gon, nitrogen Ar-W5 (5 vol.-% H2 in Ar), Ar-W2 (2 vol.-% H2 in Ar), a forming gas (5 vol.-% H2 in N2) or other noble gases, is provided at the assembling site 12 in order to prevent the metal fibers 10 from oxidizing. It can be chosen according to the material(s) of the fibers 10 if it is necessary to provide such a protective gas or not.
  • the contact points 14 of the assembled network can be distributed in an ordered or unordered manner throughout the network depending on the application of the assembled network and fix the fibers to one another. Also, the amount of contact points 14 can be chosen according the application of the network by subjecting the fibers 10 to a higher or lower pressure before carrying out steps A to C such that more or less contact points 14 are created. Also the fiber density, i.e. the amount of fibers per volume, and/or the fineness of the fibers can be used to tune the number of contact points 14.
  • Said contact points 14 also enable an electric conductivity throughout the assem bled network. Therefore, a high amount of contact points 14 can be beneficial for applications where a high electrical conductivity of the network is needed. For fil ters, on the other hand, it may not be that crucial how many contact points 14 are provided throughout the network as long as it still holds all the fibers 10 together.
  • the fibers 10, which are used for assembling a network according to the invention comprise a length of 1.0 mm or more and/or a width of 100 pm or less and/or a thickness of 50 pm or less (see Figs. 2 to 6).
  • Such fibers 10 can, for example, be produced by so called vertical or horizontal melt spinning processes, which are de scribed in documents PCT/EP2020/063026 (not yet published), WO2016/020493 A1 and WO2017/042155 A1.
  • These fibers 10 often comprise a cross-section is shaped oval, rectangular or flat in general.
  • fibers 10 which are pro prised by melt spinning often store a high amount of energy.
  • Fibers of the copper alloy (CuSi4 (4 wt .-% Si and 96 wt .-% Cu) and AISi1 (1 % by weight Si and 99% by weight Al)) have been sintered together while maintaining the flat, ribbon like, structure of the fibers.
  • the fibers were heated in an electron microscope with a heating rate of 10 K/min and a video was recorded.
  • Figure 2 shows single frames from the CuSi4 videos at special points such as the start of the sintering (to see that the sharp transitions 14 between the fibers 10 are blurred, left) and the point at which the fi bers 10 start to round off so much (right) that constrictions 15 and interruptions 16 are formed, decomposing the fibers 10.
  • the corresponding temperatures are very close to each other, which is why the highest temperature accuracy and control is necessary to achieve good results.
  • Figure 3 shows frames from a video taken with AISi1 fibers under the same condi tions as the video of Fig. 2.
  • Fig. 3 shows the same characteristic points as ex plained for Figure 2, i.e. the onset of sintering and the begin of rounding pro Deads. It could be observed that the fibers sinter together at around 602 °C, whereas at 624 °C. Further, between 602 °C and 624 °C the fibers transformed from flat ribbon like fibers towards fibers having a round cross section. This can be recognized by the fibers at 624 °C being thinner than at 602 °C. It is noted that the videos of which frames are shown in Fig.
  • the fibers 10 With classic thermal sintering using furnaces, such as resistance heated furnaces, the fibers 10 are heated with a rate of 10-20 K/min, i.e. relatively slowly. During this time, the fibers 10 undergo a so-called relaxation process and the energy stored in these fibers from their production, for example by the melt spinning pro cess, is slowly released and no longer available for forming points of connection between the metal fibers. The release of the stored energy during slow heating does not only influence the mechanical properties of the fibers 10 but also in creases the energy requirement during the actual sintering because the fibers 10 are no longer in their thermodynamic imbalance as they were after production.
  • the untreated fibers 10 as obtained from a melt spinning process and for comparison fibers 10 tempered at 300 °C for 1 hour were brought to the sinter ing temperature in a fast heating furnace (here an infrared furnace) within 1 mi nute. This temperature was held for 1 minute and then cooled as quickly as possi ble (from sintering temperature to less than 600 °C in less than 30 seconds).
  • a fast heating furnace here an infrared furnace
  • other possible heating devices are e.g. ceramic heaters or induction heaters.
  • Fibers of AISi1 had a ribbon like structure with an average length of 30 mm, an average width of 75 pm and an average thickness of 15 pm. Fibers of CuSi4 had a ribbon like structure with an average length of 20 mm, an average width of 35 pm and an average thickness of 7 pm. For these tests, the fi bers were heated within 1 min to the determined fixation temperature indicated in the table below.
  • fixation temperatures were maintained for some time, before rapidly natural cooling within 30 sec to around 500 °C and around 20 min to room temperature for CuSi4 and within 30 sec to around 330 °C and 15 min to room temperature for AISi1. After cooling the fibers were examined about whether they have a rounded cross section. Experiments were repeated with increasing fixation times at the respective fixation temperatures. The results of these tests are indi cate in the following table: One can clearly see that the higher the fixation temperature is chosen, the shorter time one has left in order to sinter the fibers 10 to one another without having them transform their outer shape. Furthermore, it can be seen that the temperature clearly depends on the material out of which the fibers 10 are made. Further the fiber size, in particular thickness and width have a certain influence on the velocity with which the cross sectional shape of the fiber transforms from flat to round. The above experiments demonstrated how the skilled person can easily determine the suitable conditions by simple trial and error for each fiber material.
  • Figure 4 shows a conventionally sintered network of previously flat fibers 10.
  • the formation of constrictions 15 and interruptions 16 of the fibers 10 can be clearly seen. Further, the cross section of the fibers was transformed from flat to round.
  • the formation of sintering necks, i.e. constrictions, corresponds to the current the ory as described in connection with Fig. 1.
  • Table 1 shows the sintering temperatures (holding time 1 min in each case) for the thermally untreated (as obtained from melt spinning) and for tempered (1 hour at 300 °C under argon atmosphere) CuSi4 fibers 10 with a ribbon like structure hav ing an average length of 20 mm, an average width of 35 pm and an average thick ness of 7 pm.
  • Table 2 analogously shows the same for AISi1 fibers 10 having an average length of 30 mm, an average width of 75 pm and an average thickness of 15 pm. Comparisons between untreated and tempered fibers were made, using a tube furnace under a protective gas atmosphere (argon) providing heating rates of 10 K/min.
  • sintering of thermally untreated CuSi4 fibers begins at significantly lower temperatures (between 890 and 910 °C) compared to the tempered fibers (begin of sintering above 950 °C) and is completed within 0.5 to 5 minutes for CuSi4 fibers and 0.5 to 5 minutes for AISi1 fibers, depending on the fixation temperature with lower fixation temperatures requiring longer fixation times.
  • Table 2 AISi1 sinter-parameters.
  • the fibers 10 experience a relaxation process before sintering temperatures can be reached, releasing stored energy too early, so it is not available for driving the sin tering process.
  • the fibers are tempered before reaching the sintering temperature. In consequence, they will behave similar to the tempered fibers reported in tables 1 and 2. The higher the energy stored in the fi bers 10 during the manufacturing process, the lower the required sintering temper ature and time can be.
  • the greatest possible energy can be introduced through high quenching rates, e.g. by the known melt spinning process. Due to the fundamental mechanisms of the process, the method according to the invention can be transferred to almost all metallic, metallic-inorganic and comparable alloys and materials, as long as suffi cient energy is stored in them.
  • Fig. 5 shows CuSi4 fibers 10 which have been sintered with the method according to the invention such that they have still retained their original flat shape.
  • Fig. 6 shows the same for AlSi 1 fibers 10. It can clearly be seen that the fibers 10 in Figs. 5 and 6 comprise an almost constant width along their length, i.e. no con striction 15 or even interruptions 16 were formed which may lead to a complete destruction of the fibers 10. That is, the width of the fibers 10 in the network ac cording to the invention does not vary more than 40%, preferably not even more than 30%.

Landscapes

  • Engineering & Computer Science (AREA)
  • Chemical & Material Sciences (AREA)
  • Manufacturing & Machinery (AREA)
  • Mechanical Engineering (AREA)
  • Textile Engineering (AREA)
  • Inorganic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Geology (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Nanotechnology (AREA)
  • Materials Engineering (AREA)
  • Electrochemistry (AREA)
  • General Chemical & Material Sciences (AREA)
  • Powder Metallurgy (AREA)
  • Nonwoven Fabrics (AREA)
  • Cell Electrode Carriers And Collectors (AREA)
  • Manufacture Of Alloys Or Alloy Compounds (AREA)
PCT/EP2021/062435 2021-05-11 2021-05-11 Network of metal fibers and method of assembling a fiber network Ceased WO2022237966A1 (en)

Priority Applications (8)

Application Number Priority Date Filing Date Title
PCT/EP2021/062435 WO2022237966A1 (en) 2021-05-11 2021-05-11 Network of metal fibers and method of assembling a fiber network
CN202280026643.6A CN117157438B (zh) 2021-05-11 2022-05-10 金属纤维网络和组装纤维网络的方法
ES22728541T ES3010516T3 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network
JP2023554284A JP2024521238A (ja) 2021-05-11 2022-05-10 金属繊維のネットワーク及び繊維ネットワークの組立方法
KR1020237036354A KR20240006512A (ko) 2021-05-11 2022-05-10 금속 섬유의 네트워크 및 섬유 네트워크의 어셈블링 방법
PCT/EP2022/062655 WO2022238413A1 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network
EP22728541.8A EP4281608B1 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network
US18/289,128 US20240367228A1 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
PCT/EP2021/062435 WO2022237966A1 (en) 2021-05-11 2021-05-11 Network of metal fibers and method of assembling a fiber network

Publications (1)

Publication Number Publication Date
WO2022237966A1 true WO2022237966A1 (en) 2022-11-17

Family

ID=75904946

Family Applications (2)

Application Number Title Priority Date Filing Date
PCT/EP2021/062435 Ceased WO2022237966A1 (en) 2021-05-11 2021-05-11 Network of metal fibers and method of assembling a fiber network
PCT/EP2022/062655 Ceased WO2022238413A1 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network

Family Applications After (1)

Application Number Title Priority Date Filing Date
PCT/EP2022/062655 Ceased WO2022238413A1 (en) 2021-05-11 2022-05-10 Network of metal fibers and method of assembling a fiber network

Country Status (7)

Country Link
US (1) US20240367228A1 (enExample)
EP (1) EP4281608B1 (enExample)
JP (1) JP2024521238A (enExample)
KR (1) KR20240006512A (enExample)
CN (1) CN117157438B (enExample)
ES (1) ES3010516T3 (enExample)
WO (2) WO2022237966A1 (enExample)

Families Citing this family (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP4624071A1 (en) 2024-03-26 2025-10-01 Max-Planck-Gesellschaft zur Förderung der Wissenschaften e.V. Metal fiber
EP4650503A1 (en) * 2024-05-15 2025-11-19 batene GmbH Three-dimensional network of metal fibers and production method

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2016020493A1 (en) 2014-08-07 2016-02-11 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Apparatus and method of manufacturing metallic or inorganic strands having a thickness in the micron range by melt spinning
WO2016075005A1 (en) * 2014-11-13 2016-05-19 Nv Bekaert Sa Sintered metal object comprising metal fibers
WO2017042155A1 (en) 2015-09-11 2017-03-16 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Apparatus and method of manufacturing metallic or inorganic fibers having a thickness in the micron range by melt spinning
WO2020016240A1 (en) * 2018-07-17 2020-01-23 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Network of metal fibers, method for producing a network of metal fibers, electrode and battery

Family Cites Families (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5102745A (en) * 1989-11-13 1992-04-07 Auburn University Mixed fiber composite structures
TW593705B (en) * 2002-02-22 2004-06-21 Hideo Nakajima Process for the production of a porous metal body
KR20090119363A (ko) * 2008-05-16 2009-11-19 주식회사 아스플로 마이크로웨이브를 이용한 금속섬유의 접합방법, 이를이용하여 제조된 금속섬유 구조체 및 금속섬유 가스필터
KR101806547B1 (ko) * 2011-04-06 2018-01-10 주식회사 제낙스 금속 섬유를 포함하는 전극 구조체를 갖는 전지 및 상기 전극 구조의 제조 방법
US20160035456A1 (en) * 2014-07-30 2016-02-04 Vorbeck Materials Corp. Electrically conductive polymer compositions
JP2019080056A (ja) * 2017-10-20 2019-05-23 キヤノン株式会社 複合磁性材料を含む磁石およびそれを用いたモータ
DE102018113340B4 (de) * 2018-06-05 2020-10-01 Otto-Von-Guericke-Universität Magdeburg Dichteoptimierte Molybdänlegierung
CN108926908B (zh) * 2018-08-15 2020-06-19 安徽东大滤材有限公司 一种耐腐高强度金属纤维毡的制备方法
CN108907186B (zh) * 2018-08-15 2019-12-06 宿州青果知识产权服务有限公司 一种增强金属纤维多孔材料强度、消音特性的烧结方法
CN109053206B (zh) * 2018-08-31 2021-07-23 中国科学院金属研究所 一种短纤维增强取向max相陶瓷基复合材料及制备方法
CN109175363B (zh) * 2018-08-31 2021-02-02 湖南惠同新材料股份有限公司 一种放电等离子烧结制备金属纤维烧结毡的方法

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2016020493A1 (en) 2014-08-07 2016-02-11 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Apparatus and method of manufacturing metallic or inorganic strands having a thickness in the micron range by melt spinning
WO2016075005A1 (en) * 2014-11-13 2016-05-19 Nv Bekaert Sa Sintered metal object comprising metal fibers
WO2017042155A1 (en) 2015-09-11 2017-03-16 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Apparatus and method of manufacturing metallic or inorganic fibers having a thickness in the micron range by melt spinning
WO2020016240A1 (en) * 2018-07-17 2020-01-23 MAX-PLANCK-Gesellschaft zur Förderung der Wissenschaften e.V. Network of metal fibers, method for producing a network of metal fibers, electrode and battery

Also Published As

Publication number Publication date
ES3010516T3 (en) 2025-04-03
JP2024521238A (ja) 2024-05-29
CN117157438B (zh) 2026-01-02
US20240367228A1 (en) 2024-11-07
EP4281608B1 (en) 2025-01-29
EP4281608C0 (en) 2025-01-29
EP4281608A1 (en) 2023-11-29
KR20240006512A (ko) 2024-01-15
CN117157438A (zh) 2023-12-01
WO2022238413A1 (en) 2022-11-17

Similar Documents

Publication Publication Date Title
KR102749409B1 (ko) 금속 섬유의 네트워크, 금속 섬유의 네트워크를 제조하기 위한 방법, 전극 및 배터리
EP4281608B1 (en) Network of metal fibers and method of assembling a fiber network
Zhang et al. The nature of reversible change in Ms temperatures of Ti–Ni alloys with alternating aging
WO2015164994A1 (zh) 一种多孔金属材料的制备方法及其应用
JP2019065312A (ja) 集電体用アルミニウム合金箔及びその製造方法
CN112376096B (zh) 一种金属材料表面微孔结构的制备方法及金属材料
WO2001046483A1 (en) Advanced alloy fiber and process of making
EP4000710A1 (en) Filter
JP4231188B2 (ja) Ni−Mn−Ga系形状記憶合金薄膜とその製造方法
JP6706258B2 (ja) 金属繊維を含む焼結金属体
JP2024521238A5 (enExample)
JPS5928626B2 (ja) 水素吸蔵用ミツシユメタル−ニツケル系四元合金の製造方法
EP0043094A1 (en) Stainless steel short fiber and process for preparing the same
JP2006028621A (ja) 水素吸蔵合金の熱処理方法
JP6223814B2 (ja) 形状記憶特性を有する金属製多孔体及びその製造方法
JP2018141209A (ja) アルミニウム合金線の製造方法
JPS5945743B2 (ja) Ag基複合電気接点素材の製造法
JP7920208B2 (ja) 電極の製造方法、電極、ドライコーティング組成物、電池、および電子回路
EP1546422A1 (en) Method of forming non-sag molybdenum-lanthana alloys
JPH1186800A (ja) タングステン線およびその製造方法、フィラメントおよびその製造方法
JPH04210834A (ja) モリブデン製金網
CN118621182A (zh) 一种镍钛形状记忆合金及其制备方法
CN113039016A (zh) 用于烃裂解的催化剂
CN121826565A (zh) 一种增材制造高体积分数γ’相镍基高温合金及其热处理方法
JPS607023B2 (ja) 無方向性薄板ばね材料の製造法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 21725158

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 21725158

Country of ref document: EP

Kind code of ref document: A1