WO2021205780A1 - 高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー - Google Patents

高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー Download PDF

Info

Publication number
WO2021205780A1
WO2021205780A1 PCT/JP2021/007969 JP2021007969W WO2021205780A1 WO 2021205780 A1 WO2021205780 A1 WO 2021205780A1 JP 2021007969 W JP2021007969 W JP 2021007969W WO 2021205780 A1 WO2021205780 A1 WO 2021205780A1
Authority
WO
WIPO (PCT)
Prior art keywords
superabsorbent polymer
polymer
acid
dehydrated
highly water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2021/007969
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
孝義 小西
坂東 健司
利夫 平岡
範朋 栗田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Unicharm Corp
Original Assignee
Unicharm Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Unicharm Corp filed Critical Unicharm Corp
Priority to EP21784575.9A priority Critical patent/EP4115973A4/en
Priority to CN202180027106.9A priority patent/CN115379892B/zh
Publication of WO2021205780A1 publication Critical patent/WO2021205780A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/30—Processes for preparing, regenerating, or reactivating
    • B01J20/34—Regenerating or reactivating
    • B01J20/3425—Regenerating or reactivating of sorbents or filter aids comprising organic materials
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/22—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof comprising organic material
    • B01J20/24—Naturally occurring macromolecular compounds, e.g. humic acids or their derivatives
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/22—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof comprising organic material
    • B01J20/26—Synthetic macromolecular compounds
    • B01J20/264—Synthetic macromolecular compounds derived from different types of monomers, e.g. linear or branched copolymers, block copolymers, graft copolymers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/22—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof comprising organic material
    • B01J20/26—Synthetic macromolecular compounds
    • B01J20/265—Synthetic macromolecular compounds modified or post-treated polymers
    • B01J20/267—Cross-linked polymers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/28—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof characterised by their form or physical properties
    • B01J20/28002—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof characterised by their form or physical properties characterised by their physical properties
    • B01J20/28011—Other properties, e.g. density, crush strength
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/30—Processes for preparing, regenerating, or reactivating
    • B01J20/3085—Chemical treatments not covered by groups B01J20/3007 - B01J20/3078
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J20/00—Solid sorbent compositions or filter aid compositions; Sorbents for chromatography; Processes for preparing, regenerating or reactivating thereof
    • B01J20/30—Processes for preparing, regenerating, or reactivating
    • B01J20/34—Regenerating or reactivating
    • B01J20/345—Regenerating or reactivating using a particular desorbing compound or mixture
    • B01J20/3475—Regenerating or reactivating using a particular desorbing compound or mixture in the liquid phase
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J2220/00—Aspects relating to sorbent materials
    • B01J2220/50—Aspects relating to the use of sorbent or filter aid materials
    • B01J2220/68—Superabsorbents
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02W—CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT
    • Y02W30/00—Technologies for solid waste management
    • Y02W30/50—Reuse, recycling or recovery technologies
    • Y02W30/62—Plastics recycling; Rubber recycling

Definitions

  • the present disclosure relates to a method for producing a superabsorbent polymer recycled from a used superabsorbent polymer, and a superabsorbent polymer recycled from a used superabsorbent polymer.
  • Patent Document 1 discloses the following method for regenerating a water-absorbent resin.
  • a method for regenerating a water-absorbent resin in which a water-absorbent resin that has absorbed a liquid to be absorbed is taken out from a used body fluid-absorbing article and washed and dehydrated. The washing and / or dehydration treatment is absorbed by the water-absorbent resin.
  • a method for regenerating a water-absorbent resin which comprises an operation of placing the liquid to be absorbed in an environment for discharging the liquid to be absorbed.
  • Patent Document 1 cleans and / or dehydrates the water-absorbent resin that has absorbed the absorbed liquid, but does not dehydrate all the absorbed liquid from the water-absorbent resin. Therefore, the regenerated water-absorbing resin is used. The resin tends to exhibit the color of the liquid to be absorbed. Further, in the method described in Patent Document 1, when the drying step is performed to obtain the regenerated water-absorbent resin, the water-absorbent resins stick to each other, so that the method is described in Examples of Reference 1. In addition, a crushing process and a classification process are required.
  • the present disclosure is a highly water-absorbent recycled polymer capable of suppressing the adhesion of particles to each other, efficiently drying each particle, and producing a highly water-absorbent recycled polymer having excellent whiteness. It is an object of the present invention to provide a manufacturing method.
  • the present disclosures are a method for producing a superabsorbent polymer regenerated from a used superabsorbent polymer, in which the used superabsorbent polymer is dehydrated to obtain a dehydrated superabsorbent polymer.
  • the particles of the superabsorbent polymer are attached to the dehydrated superabsorbent polymer to form the superabsorbent polymer to which the particles are attached, and the dehydrated superabsorbent polymer is retained.
  • a method comprising a particle group attachment step of allowing the water to be absorbed by the particle group, and a drying step of drying the superabsorbent polymer to which the particle group is attached to form the superabsorbent polymer. I found it.
  • the method for producing a highly water-absorbent recycled polymer of the present disclosure can prevent particles from sticking to each other, efficiently dry each particle, and produce a highly water-absorbent recycled polymer having excellent whiteness. ..
  • a method for producing a super absorbent polymer recycled from a used superabsorbent polymer A dehydration step of dehydrating the used superabsorbent polymer to form a dehydrated superabsorbent polymer, The particles of the superabsorbent polymer are attached to the dehydrated superabsorbent polymer to form the superabsorbent polymer to which the particles are attached, and the moisture retained by the dehydrated superabsorbent polymer is retained.
  • Particle group attachment step to be absorbed by the above particle group
  • the above method which comprises.
  • the production method includes a predetermined dehydration step, a particle swarm adhesion step, and a drying step.
  • the particles of the superabsorbent polymer adhere to the dehydrated superabsorbent polymer and absorb the water retained by the dehydrated superabsorbent polymer. Further, the surface area of the superabsorbent polymer particles is increased by adhering to the dehydrated superabsorbent polymer. Therefore, in the above-mentioned production method, it is possible to efficiently dry each particle and efficiently form a highly water-absorbent recycled polymer while suppressing the particles from sticking to each other in the above-mentioned drying step.
  • suppressing the adhesion between particles may be referred to as "adhesion inhibitory property”
  • efficiently drying each particle may be referred to as "efficiency drying property”.
  • the highly water-absorbent recycled polymer since the highly water-absorbent recycled polymer has particles adhering to its surface, it easily reflects light diffusely, has excellent whiteness, and makes the user feel clean and reassuring to the user. It can make you feel.
  • the super absorbent polymer recycled from the used superabsorbent polymer is often colored in the color of the liquid absorbed during use. For example, when the used superabsorbent polymer absorbs excrement, the used superabsorbent polymer is often colored brown. In such a case, the super absorbent polymer formed from the used superabsorbent polymer often remains colored in brown.
  • the highly water-absorbent recycled polymer has a predetermined whiteness W and a predetermined yellowness YI, so that the whiteness is excellent and the user can feel a sense of cleanliness.
  • a dehydrated superabsorbent polymer is formed by contacting with a salt, acid or base in the dehydration step. Therefore, the dehydrated superabsorbent polymer tends to have a high solidity ratio, and in the particle group attachment step, the particles of the superabsorbent polymer are easily attached to the dehydrated superabsorbent polymer, and the drying step is performed. It is excellent in sticking inhibitory property and efficient drying property.
  • the used superabsorbent polymer in the dehydration step, is brought into contact with a predetermined salt, and the used superabsorbent polymer is dehydrated using the difference in osmotic pressure. Therefore, the above-mentioned production method can form a dehydrated superabsorbent polymer having a high solidity ratio. In addition, the solid content of the dehydrated superabsorbent polymer tends to be high. As a result, in the particle group attachment step, the particles of the superabsorbent polymer are easily attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property.
  • the used superabsorbent polymer contains an acid group, and in the dehydration step, the used superabsorbent polymer is immersed in an aqueous solution containing the base to form the dehydrated superabsorbent polymer.
  • a used superabsorbent polymer in the dehydration step, is dehydrated using an aqueous solution containing an alkali metal hydroxide. Therefore, since a part of the acid group and its salt (particularly calcium salt) contained in the used superabsorbent polymer forms an alkali metal salt, the superabsorbent polymer, particularly the used superabsorbent polymer, has a high water absorption. The part derived from the polymer has excellent water absorption. In addition, the solid content of the dehydrated superabsorbent polymer tends to be high. As a result, in the particle group attachment step, the particles of the superabsorbent polymer are easily attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property.
  • a dehydrated superabsorbent polymer is formed using an aqueous solution containing a predetermined acid. Therefore, the acid group of the used superabsorbent polymer tends to have a free acid group from the salt thereof, and the solidity ratio of the dehydrated superabsorbent polymer tends to increase. As a result, in the particle group attachment step, the particles of the superabsorbent polymer are easily attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property.
  • the dehydrated superabsorbent polymer has a predetermined solid content in the dehydration step. Therefore, in the particle group attachment step, the particles of the superabsorbent polymer are easily attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property.
  • the drying step is excellent in sticking inhibitory property and efficient drying property.
  • the particles of the superabsorbent polymer have a predetermined solid ratio in the particle group attachment step, the particles of the superabsorbent polymer are added to the dehydrated superabsorbent polymer in the particle group attachment step. Is easy to adhere, and the drying step is easy to be excellent in sticking inhibitory property and efficient drying property.
  • the particle group of the superabsorbent polymer contains a predetermined amount of particles having a predetermined particle size in the particle group attachment step
  • the dehydrated superabsorbent polymer has high water absorption in the particle group attachment step.
  • the particles of the sex polymer are easily attached, and the drying step is excellent in sticking inhibitory property and efficient drying property.
  • the highly water-absorbent recycled polymer has a particle group containing a predetermined amount of particles having a predetermined particle size on its surface, light is easily diffusely reflected and the whiteness is excellent.
  • the superabsorbent polymer to which the particle group is attached is dried under predetermined conditions in the drying step, it is possible to suppress coloring, discoloration, etc. of the superabsorbent recycled polymer.
  • the used superabsorbent polymer is contained in used hygiene products, including pulp fibers.
  • the above dehydration step is the next sub-step, A superabsorbent polymer obtained by primary dehydrating a mixture containing the used superabsorbent polymer and the pulp fiber from the used superabsorbent polymer having a solid content of 2.0 to 9.0% by mass.
  • a primary dehydration substep that separates the primary dehydrated superabsorbent polymer from the pulp fibers while primary dehydrating so that
  • a secondary dehydration substep which dehydrates the primary dehydrated superabsorbent polymer so as to form a secondary dehydrated superabsorbent polymer having a solids content of 10.0 to 40.0% by mass.
  • the method according to any one of aspects 1 to 11, which comprises.
  • the dehydration step includes a primary dehydration substep and a secondary dehydration substep.
  • the primary dehydration substep in order to form a primary dehydrated superabsorbent polymer having a predetermined solidity from the primary dehydrated superabsorbent polymer, the primary dehydration is performed from the constituent materials constituting the sanitary goods. It becomes easy to separate the superabsorbent polymer and the mixture of the pulp fibers. Further, in the separated mixture, the primary dehydrated superabsorbent polymer and the pulp fiber are separated from each other, and the primary dehydrated superabsorbent polymer can be easily taken out.
  • a secondary dehydrated superabsorbent polymer (dehydrated superabsorbent polymer) having a predetermined solidity is formed from the primary dehydrated superabsorbent polymer. Therefore, the water retained by the primary dehydrated superabsorbent polymer can be discharged to purify the superabsorbent polymer, and in the particle group attachment step, the dehydrated superabsorbent polymer has high water absorbency.
  • the drying step tends to be excellent in sticking inhibitory property and efficient drying property.
  • a super absorbent polymer recycled from a used superabsorbent polymer has a superabsorbent polymer recovered from the used superabsorbent polymer and a particle group of the superabsorbent polymer linked to the surface of the superabsorbent polymer.
  • the highly water-absorbent recycled polymer has a whiteness (W) of 80 or more and a yellowness (YI) of 20 or less. The above-mentioned highly water-absorbent recycled polymer.
  • the superabsorbent polymer has a particle group of superabsorbent polymer linked to its surface, and has a predetermined whiteness W and a yellowness YI of 20 or less. Therefore, the highly water-absorbent recycled polymer is excellent in whiteness, and can make the user feel clean and feel secure.
  • a method for producing a superabsorbent polymer regenerated from a used superabsorbent polymer of the present disclosure (hereinafter, may be referred to as a "method for producing a superabsorbent polymer"), and a used superabsorbent polymer.
  • the super absorbent polymer recycled from the polymer (hereinafter, may be referred to as “super absorbent polymer”) will be described in detail below.
  • the method for producing a highly water-absorbent recycled polymer of the present disclosure includes the following steps. -A dehydration step of dehydrating the used superabsorbent polymer to form a dehydrated superabsorbent polymer (hereinafter, may be referred to as a "dehydration step”). -The particles of the superabsorbent polymer are attached to the dehydrated superabsorbent polymer to form the superabsorbent polymer to which the particles are attached, and the moisture retained by the dehydrated superabsorbent polymer is formed. Is absorbed by the above particle group (hereinafter, may be referred to as “particle group adhesion step”). -A drying step of drying the superabsorbent polymer to which the particle group is attached to form the superabsorbent recycled polymer (hereinafter, may be referred to as a "drying step").
  • the used superabsorbent polymer is dehydrated to form the dehydrated superabsorbent polymer.
  • the used superabsorbent polymer is not particularly limited as long as it absorbs a liquid, and examples thereof include superabsorbent polymers contained in used hygiene products.
  • the sanitary products include disposable diapers, urine absorbing pads, disposable shorts, sanitary napkins, panty liners, bed sheets, pet sheets and the like.
  • the above-mentioned used hygiene products are hygiene products used by the user, hygiene products that have absorbed the user's excrement, and hygiene products used by the user, and are the user's excrement. Includes hygiene products that do not absorb hygiene products, unused and discarded hygiene products (for example, hygiene products in which a highly water-absorbent polymer absorbs a treatment solution for recycling hygiene products).
  • composition of the superabsorbent polymer examples include those known in the technical field of hygiene products, and examples thereof include starch-based, cellulosic-based, and synthetic polymer-based superabsorbent polymers.
  • starch-based or cellulose-based highly water-absorbent polymer examples include a starch-acrylic acid (salt) graft copolymer, a saponified product of a starch-acrylonitrile copolymer, and a crosslinked product of sodium carboxymethyl cellulose.
  • Examples of the synthetic polymer superabsorbent polymer include polyacrylate-based, polysulfonate-based, maleate anhydride-based, polyacrylamide-based, polyvinyl alcohol-based, polyethylene oxide-based, polyaspartate-based, and polyglutamic acid. Examples thereof include salt-based, polyarginate-based, starch-based, and cellulose-based super absorbent polymers (SAP, Super Absorbent Polymer).
  • the superabsorbent polymer can be divided into those having an acid group (for example, a carboxyl group or a sulfo group) and those having no acid group.
  • Examples of the method for dehydrating a used superabsorbent polymer include methods known in the art, such as salts, acids, bases, hydrophilic organic solvents, temperature changes, and water absorbents.
  • the dehydrated superabsorbent polymer can be dehydrated so as to have a predetermined solid ratio.
  • the predetermined solid content is preferably 10.0% by mass or more, more preferably 20.0% by mass or more, and further preferably 30.0% by mass or more.
  • the predetermined solid content is preferably 50.0% by mass or less, and more preferably 40.0% by mass or less.
  • the used superabsorbent polymer can be dehydrated by immersing it in the salt itself or an aqueous solution containing the salt (for example, a saturated aqueous solution).
  • the salt include a base and a salt such as an acid.
  • the base include hydroxides of alkali metals (for example, lithium, sodium and potassium), hydroxides of alkaline earth metals (for example, beryllium, magnesium, calcium, strontium and barium) and the like.
  • alkali metal hydroxide examples include lithium hydroxide, sodium hydroxide and potassium hydroxide, and any combination thereof.
  • hydroxide of the alkaline earth metal examples include beryllium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, and any combination thereof.
  • the base is preferably an alkali metal hydroxide. This is from the viewpoint of making it difficult to inhibit the water absorption of the highly water-absorbent recycled polymer.
  • the acid is not particularly limited, and examples thereof include an inorganic acid and an organic acid.
  • the inorganic acid include sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, boric acid, bromic acid, and iodic acid.
  • the organic acid include those having an acid group, for example, a carboxyl group, a sulfo group, and the like.
  • An organic acid having a sulfo group is called a sulfonic acid
  • an organic acid having a carboxyl group and no sulfo group is called a carboxylic acid.
  • the organic acid is preferably an organic acid having a carboxyl group, particularly a carboxylic acid, from the viewpoint of protecting the equipment.
  • the organic acid When the organic acid has a carboxyl group, the organic acid can have one or more carboxyl groups per molecule, and preferably has a plurality of carboxyl groups. By doing so, the organic acid easily forms a chelate complex with a divalent or higher valent metal contained in excrement or the like, for example, calcium, and it becomes difficult to inhibit the water absorption of the highly water-absorbent recycled polymer. This is because the effect of making it easier to reduce the ash content of recycled pulp fibers produced from sanitary goods can be obtained.
  • a divalent or higher valent metal contained in excrement or the like for example, calcium
  • organic acid examples include citrate, tartaric acid, malic acid, succinic acid, oxalic acid (these are carboxylic acids having a plurality of carboxyl groups), gluconic acid (C6), pentanoic acid (C5), and butanoic acid (C4). ), Propionic acid (C3), glycolic acid (C2), acetic acid (C2), for example, glacial acetic acid, formic acid (C1), lactic acid (above, carboxylic acid having one carboxyl group), methanesulfonic acid, trifluoromethanesulfon. Acids, benzenesulfonic acids, p-toluenesulfonic acids (above, sulfonic acids) and the like can be mentioned.
  • the acid is an acid having a larger acid dissociation constant (pK a, in water) of the acid group in the highly water-absorbent polymer. It may be an acid having a dissociation constant (pK a, in water).
  • pK a in water
  • the acid group of the superabsorbent polymer tends to form a salt (for example, an alkali metal salt), and the superabsorbent polymer described later has an excellent water absorption ratio and water retention ratio.
  • the acid has a plurality of acid groups
  • a (in water) is preferably larger than the acid dissociation constant (pK a , in water) of the acid group of the highly water-absorbent polymer, and when the highly water-absorbent polymer has multiple acid groups, the above acid acid dissociation constant (pK a, water) smallest acid dissociation constant (pK a, water) of is larger than the largest acid dissociation constant of the plurality of types of acid groups of the superabsorbent polymer (pK a, water) Is preferable.
  • a salt for example, an alkali metal salt
  • the acid dissociation constant (pk a, water) can be employed a value according to the electrochemical Handbook of Electrochemical Society edit. According to the electrochemical Handbook, acid dissociation constant of the major compounds (pk a, water, 25 ° C.) are as follows. [Organic acid] -Tartaric acid: 2.99 (pK a1 ), 4.44 (pK a2 ) -Malic acid: 3.24 (pK a1 ), 4.71 (pK a2 ) -Citric acid: 2.87 (pK a1 ), 4.35 (pK a2 ), 5.69 (pK a3 ) [Inorganic acid] -Sulfuric acid: 1.99 (pK a2 )
  • Acid dissociation constant of the acid is not described in electrochemical Handbook (pk a, water) can be determined by measurement.
  • Carbonic acid as the acid is preferable because carbonic acid does not easily remain in the aqueous solution or can be easily removed by heating or the like. Further, the above-mentioned acids other than carbonic acid have antibacterial properties against, for example, a highly water-absorbent recycled polymer in a wet state, a highly water-absorbent recycled polymer in a dry state, and the like when the highly water-absorbent recycled polymer in a wet state is at an acidic pH. Can be given.
  • Examples of the salt include lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium chloride, sodium chloride, potassium chloride and the like.
  • the salt itself is preferably used as the salt itself or as an aqueous solution, and the salt itself is preferable.
  • the aqueous solution is preferably a saturated aqueous solution.
  • the used superabsorbent polymer can be dehydrated by immersing it in an aqueous solution containing an acid in the dehydration step. can.
  • the acid the acid having an acid dissociation constant of the acid groups in the superabsorbent polymer (pK a, water) smaller acid dissociation constant than (pK a, water) (hereinafter sometimes referred to as "predetermined strong acid” ) Is preferable. This is from the viewpoint of the efficiency of dehydration of the used superabsorbent polymer.
  • the acid dissociation constant (pK a , in water) of the acid having the largest acid dissociation constant (pK a) is the largest.
  • the acid dissociation constant (pK a , in water) of the acid group of the highly water-absorbent polymer is preferably smaller than the acid dissociation constant (pK a , in water) of the acid group of the highly water-absorbent polymer, and when the highly water-absorbent polymer has multiple acid groups, the above acid acid dissociation constant (pK a, water) the largest acid dissociation constant of (pK a, water) is smaller than the smallest acid dissociation constant of the plurality of types of acid groups of the superabsorbent polymer (pK a, water) Is preferable. This is from the viewpoint of the efficiency of dehydration of the super absorbent polymer.
  • predetermined strong acid examples include the acids described in the section on salts, such as sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid.
  • the aqueous solution containing the acid preferably has a predetermined pH, and the predetermined pH is preferably 4.5 or less, more preferably 4.0 or less, still more preferably 3.5 or less, and even more preferably. It is 3.0 or less.
  • the dehydrated superabsorbent polymer tends to have the above-mentioned predetermined solid ratio.
  • the predetermined pH is preferably 0.5 or more, and more preferably 1.0 or more. If the predetermined pH is too low, the acid group of the superabsorbent polymer tends to change from a salt state (for example, a sodium salt) to a free acid state, and the water absorbency of the superabsorbent polymer is lowered. In some cases.
  • a salt state for example, a sodium salt
  • pH means a value at 25 ° C. Further, the pH can be measured using, for example, a twin pH meter AS-711 manufactured by HORIBA, Ltd.
  • the used superabsorbent polymer is dehydrated and dehydrated by stirring the used superabsorbent polymer in an aqueous solution containing an acid for about 5 to 60 minutes, depending on the temperature.
  • a water-absorbent polymer can be formed.
  • the acid group of the superabsorbent polymer having an acid group tends to change from the salt (for example, sodium salt) state to the free acid state, so that the water absorbency of the superabsorbent polymer is reduced.
  • the water absorption was superabsorbent polymer, when placed in an aqueous solution containing an acid, negatively charged hydrophilic group (e.g., -COO -) is neutralized by the charged hydrogen ions positively (H +) (e.g., -COOH), the ion repulsive force of the hydrophilic group is weakened, the water absorption capacity is reduced, and the superabsorbent polymer is dehydrated.
  • negatively charged hydrophilic group e.g., -COO -
  • H + charged hydrogen ions positively
  • H + e.g., -COOH
  • the temperature of the aqueous solution containing the acid in the dehydration step is not particularly limited and can be, for example, room temperature (25 ° C.) and may be higher than room temperature.
  • the temperature of the aqueous solution containing the acid in the dehydration step is preferably higher than room temperature, more preferably 60 to 100 ° C, still more preferably 70 to 95 ° C, and even more preferably 80 to 90 ° C. ..
  • the acid contained in the acid-containing aqueous solution facilitates sterilization of bacteria derived from excrement and the like contained in the acid-containing aqueous solution.
  • the used superabsorbent polymer can be dehydrated by immersing it in an aqueous solution containing a base in the dehydration step. can.
  • an acid group for example, a carboxyl group or a sulfo group
  • Examples of the base include hydroxides of alkali metals (for example, lithium, sodium and potassium) and hydroxides of alkaline earth metals (for example, beryllium, magnesium and potassium) described in the section of "salt". , Alkali metals (eg, lithium, sodium, potassium) hydroxides are preferred.
  • the acid group of the superabsorbent polymer particularly the portion derived from the used superabsorbent polymer, forms a salt, and the portion derived from the used superabsorbent polymer, and thus the superabsorbent polymer, is recycled.
  • the polymer tends to have excellent water absorption.
  • the aqueous solution containing the base preferably has a predetermined pH, and the predetermined pH is preferably 8.0 or more, more preferably 9.0 or more, and further preferably 10.0 or more.
  • the predetermined pH is preferably 14.0 or less, and more preferably 13.0 or less.
  • the pH measurement method is as described above.
  • the hydrophilic organic solvent is preferably miscible with water, and is, for example, an alcohol solvent (for example, methanol, ethanol, propyl alcohol and its isomer, butyl alcohol and its isomer), and a ketone solvent.
  • an alcohol solvent for example, methanol, ethanol, propyl alcohol and its isomer, butyl alcohol and its isomer
  • a ketone solvent examples thereof include a solvent (for example, acetone, methyl ethyl ketone), a nitrile solvent (for example, acetonitrile) and the like.
  • the dehydration step is as follows: Can include substeps of. A mixture containing the used superabsorbent polymer and the pulp fiber is formed from the used superabsorbent polymer so as to form a primary dehydrated superabsorbent polymer having a predetermined solid ratio.
  • the primary dehydration substep / primary dehydrated superabsorbent polymer that separates the predetermined primary dehydrated superabsorbent polymer and the pulp fiber while the secondary dehydration is performed is secondary to have a predetermined solid ratio.
  • the pulp fiber is easily separated from the primary dehydrated superabsorbent polymer, and the primary dehydrated superabsorbent polymer is easily separated from the pulp fiber.
  • the particles of the superabsorbent polymer are likely to be attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property.
  • the predetermined solid content of the primary dehydrated superabsorbent polymer is preferably 2.0 to 9.0% by mass, more preferably 3.0 to 9.0% by mass, and even more preferably 3.0 to 9. It is 0.0% by mass.
  • the predetermined solid content of the secondary dehydrated superabsorbent polymer is preferably 10.0 to 40.0% by mass, more preferably 11.0 to 35.0% by mass, and even more preferably 12.0 to 30%. It is 0.0% by mass.
  • the solidity ratio of the primary dehydrated superabsorbent polymer and the solidity ratio of the secondary dehydrated superabsorbent polymer (dehydrated superabsorbent polymer) are the above-mentioned salts, acids, bases, and hydrophilic organic solvents. , Temperature change, type of water absorbent, time of immersion in them, etc. can be adjusted.
  • ⁇ Particle group adhesion step In the particle group attachment step, the particles of the superabsorbent polymer are attached to the dehydrated superabsorbent polymer to form the superabsorbent polymer to which the particles are attached, and the dehydrated superabsorbent polymer is retained. The water is absorbed by the particle group.
  • the composition of the superabsorbent polymer particle group is not particularly limited, and can have a composition similar to that of the superabsorbent polymer (used superabsorbent polymer), and can have the same composition as the superabsorbent polymer described above. It can have the same or different composition as the polymer (used super absorbent polymer).
  • the specific composition of the particles of the superabsorbent polymer is as described in the section “Dehydration step”, and thus the description thereof will be omitted here.
  • the particle group of the super absorbent polymer is preferably unused. This is from the viewpoint of the whiteness of the highly water-absorbent recycled polymer.
  • the particle group of the superabsorbent polymer can be fine powder generated when the superabsorbent polymer is produced and fine powder recovered when the sanitary product is produced.
  • the fine powder generated during the production of the superabsorbent polymer includes the fine powder produced during the pulverization of the bulk polymer, the emulsion polymer, the solution polymer, the fine powder produced during the granulation of the reverse phase suspension polymer, and the like. And so on.
  • Examples of the fine powder collected during the production of the sanitary product include fine powder collected by a dust collector.
  • the particle group of the super absorbent polymer preferably has a solid content of 90.0% by mass or more, and more preferably 95.0% by mass or more.
  • the particles of the superabsorbent polymer adhere to the dehydrated superabsorbent polymer, and it becomes easier to absorb the water, and the drying step has a sticking inhibitory property and efficient drying property. It becomes easy to be excellent.
  • the upper limit of the solid content of the particles of the super absorbent polymer is 100.0% by mass.
  • the method for measuring the solidity ratio is as described above.
  • the particle group of the superabsorbent polymer preferably has a particle size smaller than that of the dehydrated superabsorbent polymer, more preferably 300 ⁇ m or less, still more preferably 200 ⁇ m or less, and even more preferably 150 ⁇ m or less. Has a particle size of. Further, the particle group of the super absorbent polymer preferably has a particle size of more than 1 ⁇ m, more preferably more than 30 ⁇ m, still more preferably more than 45 ⁇ m, and even more preferably more than 50 ⁇ m.
  • the particle size of the dehydrated superabsorbent polymer described above means the particle size of the dehydrated superabsorbent polymer after being dried at 50 ° C. for 180 minutes.
  • particles having a particle size within the upper and lower limit ranges are preferably 60% by mass or more, more preferably 70% by mass or more, still more preferably 80% by mass or more. And even more preferably, it is contained in a mass ratio of 90% by mass or more. Further, the particle group of the super absorbent polymer can contain particles having a particle size within the upper and lower limit ranges in a mass ratio of 100% by mass or less.
  • the particles of the superabsorbent polymer are excellent in handleability. Further, in the particle group attachment step, the particles of the superabsorbent polymer are likely to be attached to the dehydrated superabsorbent polymer, and the drying step is likely to be excellent in sticking inhibitory property and efficient drying property. In addition, the highly water-absorbent recycled polymer tends to reflect light diffusely and has excellent whiteness.
  • the mass ratio of particles having a predetermined particle size with respect to the superabsorbent polymer particle group and the superabsorbent recycled polymer is the nominal opening specified in JIS Z 8801-1 according to ISO 17190-3. It can be measured as follows using a sieve having. (1) A sieve having a nominal opening of the lower limit of the particle size of the sample to be measured (hereinafter referred to as “lower limit sieve”) and a sieve having a nominal opening of the upper limit of the particle size of the sample to be measured (hereinafter referred to as “lower limit sieve"). Hereinafter referred to as "upper limit sieve”) is prepared. For example, when measuring the amount of particles having a particle size of 45 to 300 ⁇ m in a sample, a lower limit sieve having a nominal opening of 45 ⁇ m and an upper sieve having a nominal opening of 300 ⁇ m are prepared.
  • Mass of sample to be measured m 3 (g), for example, 100 g is precisely measured.
  • the particles of the superabsorbent polymer are preferably 50 to 150 parts by mass, more preferably 60 to 120 parts by mass, and even more preferably 100 parts by mass with respect to 100 parts by mass of the dehydrated superabsorbent polymer. Mix at a ratio of 70 to 100 parts by mass. As a result, the next drying step tends to be excellent in sticking inhibitory property and efficient drying property. In addition, the highly water-absorbent recycled polymer tends to be excellent in whiteness.
  • the superabsorbent polymer to which the particle group is attached preferably has a solid content of 30.0% by mass or more, more preferably 35.0% by mass or more, and even more preferably 40.0% by mass or more.
  • the superabsorbent polymer to which the particle group is attached preferably has a solid content of 90.0% by mass or less.
  • the superabsorbent polymer to which the particles are attached is dried to form a superabsorbent recycled polymer.
  • the super absorbent polymer to which the particle group is attached is dried at a drying temperature of, for example, 80 to 150 ° C., preferably 100 to 120 ° C. As a result, coloring is suppressed in a short drying time, and it becomes easy to form a highly water-absorbent recycled polymer having excellent water absorption.
  • the acid groups of the highly water-absorbent recycled polymer undergo dehydration condensation, which reduces the water absorption of the highly water-absorbent recycled polymer and may cause the highly water-absorbent recycled polymer to be colored brown. be.
  • the superabsorbent polymer to which the particle group is attached can be dried for a drying time of, for example, 30 to 300 minutes, preferably 60 to 180 minutes. If the drying time is short, the solidity ratio of the highly water-absorbent recycled polymer formed may be low, depending on the drying temperature. If the drying time is long, the acid groups of the highly water-absorbent recycled polymer may undergo dehydration condensation, and the water absorption of the highly water-absorbent recycled polymer may decrease, depending on the drying temperature.
  • the drying step may be carried out under reduced pressure, for example, at 0.1 kPa or more and less than 100 kPa.
  • the highly water-absorbent recycled polymer preferably has a particle size of more than 250 ⁇ m, more preferably more than 300 ⁇ m, and even more preferably more than 350 ⁇ m.
  • the superabsorbent polymer to which the particle group is attached preferably has a particle size of 800 ⁇ m or less, more preferably 750 ⁇ m or less, and even more preferably 700 ⁇ m or less.
  • the highly water-absorbent recycled polymer preferably contains particles having a particle size within the upper and lower limit ranges of 60% by mass or more, more preferably 70% by mass or more, still more preferably 80% by mass or more, and further. More preferably, it is contained in a mass ratio of 90% by mass or more. Further, the highly water-absorbent recycled polymer can contain particles having a particle size within the upper and lower limit ranges in a mass ratio of 100% by mass or less. As a result, the super absorbent polymer can be easily reused in various applications in which the superabsorbent polymer is used, for example, hygiene products.
  • the highly water-absorbent recycled polymer preferably has a solid content of 90.0% by mass or more, and more preferably 95.0% by mass or more. Further, the highly water-absorbent recycled polymer preferably has a solid content of 100.0% by mass or less. As a result, the highly water-absorbent recycled polymer is less likely to adhere and is more likely to have excellent water absorption.
  • the method for measuring the solidity ratio is as described above.
  • the highly water-absorbent recycled polymer preferably has a whiteness (W) of 80 or more, more preferably 82 or more, and even more preferably 84 or more. Thereby, the highly water-absorbent recycled polymer is excellent in whiteness, and the user can feel a sense of cleanliness.
  • the highly water-absorbent recycled polymer preferably has a yellowness (YI) of 20 or less, more preferably 19 or less, and even more preferably 18 or less.
  • YI yellowness
  • the highly water-absorbent recycled polymer is excellent in whiteness, and the user can feel a sense of cleanliness.
  • the whiteness (W) and the yellowness (YI) are measured as follows.
  • (1) Prepare an illumination metering type color difference meter Z-300A manufactured by Nippon Denshoku Kogyo Co., Ltd. in a constant temperature and humidity chamber with a temperature of 20 ⁇ 5 ° C. and a humidity of 65 ⁇ 5% RH.
  • (2) Spread 4.5 g of the highly water-absorbent recycled polymer evenly on the glass window (diameter 40 mm) of the sample table of the color difference meter.
  • the highly water-absorbent recycled polymer preferably has a water absorption ratio of 30 times (g / g) or more, more preferably 40 times (g / g) or more, and 45 times (g / g) or more.
  • the highly water-absorbent recycled polymer preferably has a water absorption ratio of 80 times (g / g) or less, and more preferably 70 times (g / g) or less. This is from the viewpoint of water absorption and shape retention of the highly water-absorbent recycled polymer.
  • the water absorption ratio is measured as follows. (1) Prepare a bag (200 mm ⁇ 200 mm) made of nylon net (250 mesh nylon net manufactured by NBC Meshtec Inc.), and measure its mass: N 0 (g). (2) Put about 5 g of a sample in a nylon net bag and measure the mass including the nylon net bag: A 0 (g). (3) Put 1 L of physiological saline in a beaker, immerse the prepared nylon net bag containing the sample, and let stand for 3 minutes.
  • the highly water-absorbent recycled polymer preferably has a water retention ratio of 20 times (g / g) or more, more preferably 25 times (g / g) or more, and 30 times (g / g) or more.
  • the highly water-absorbent recycled polymer preferably has a water retention ratio of 50 times (g / g) or less, and more preferably 45 times (g / g) or less. This is from the viewpoint of water retention and shape retention of the highly water-absorbent recycled polymer.
  • the superabsorbent polymer produced by the production method of the present disclosure can be used without limitation in the fields in which the superabsorbent polymer is used, and examples thereof include the field of hygiene products.
  • the hygienic products are not particularly limited, and examples thereof include disposable diapers, disposable shorts, sanitary napkins, panty liners, urine absorbing pads, bed sheets, pet sheets and the like.
  • Example 1 ⁇ Dehydration step> Super absorbent polymer No. that absorbed water from the absorber of used disposable diapers. A mixture of 1 (polyacrylate-based SAP) and pulp fiber was taken out. In the above mixture, the water-absorbed superabsorbent polymer No. 1 and the pulp fiber are integrated, and it was difficult to separate them. In addition, the water-absorbed superabsorbent polymer No. 1 and the pulp fiber were colored brownish.
  • the above mixture was immersed in a dilute sulfuric acid aqueous solution having a pH of 2.0 for 10 minutes to dehydrate the superabsorbent polymer to form a primary dehydrated superabsorbent polymer.
  • Primary dehydrated super absorbent polymer No. 1 and the pulp fiber were easily separated from each other.
  • the primary dehydrated superabsorbent polymer No. 1 and pulp fiber were separated.
  • Primary dehydrated super absorbent polymer No. When 1 was recovered and the solid content thereof was measured according to the method described in this specification, it was 15% by mass.
  • Primary dehydrated super absorbent polymer No. 1 was held in a container filled with particles of sodium sulfate itself for 30 minutes. Primary dehydrated super absorbent polymer No. Sodium sulfate that had absorbed the liquid was attached to the surface of No. 1. Primary dehydrated super absorbent polymer No. The superabsorbent sodium sulfate adhering to the surface of No. 1 was removed by a sieve, and the superabsorbent polymer No. 1 was secondarily dehydrated. 1 was formed. Secondary dehydrated super absorbent polymer No. When 1 was recovered and the solid content thereof was measured according to the method described in this specification, it was 20% by mass. Secondary dehydrated super absorbent polymer No. No. 1 was colored light brown.
  • the superabsorbent polymer No. 1 polyacrylate-based SAP, particle size: 100% by mass, more than 50 ⁇ m and 150 ⁇ m or less, solidity: 98% by mass

Landscapes

  • Chemical & Material Sciences (AREA)
  • Analytical Chemistry (AREA)
  • Organic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Solid-Sorbent Or Filter-Aiding Compositions (AREA)
  • Processes Of Treating Macromolecular Substances (AREA)
  • Separation, Recovery Or Treatment Of Waste Materials Containing Plastics (AREA)
  • Absorbent Articles And Supports Therefor (AREA)
PCT/JP2021/007969 2020-04-10 2021-03-02 高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー Ceased WO2021205780A1 (ja)

Priority Applications (2)

Application Number Priority Date Filing Date Title
EP21784575.9A EP4115973A4 (en) 2020-04-10 2021-03-02 Method for producing highly water-absorbing recycled polymer, and highly water-absorbing recycled polymer
CN202180027106.9A CN115379892B (zh) 2020-04-10 2021-03-02 高吸水性再循环聚合物的制造方法和高吸水性再循环聚合物

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2020-071221 2020-04-10
JP2020071221A JP7481151B2 (ja) 2020-04-10 2020-04-10 高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー

Publications (1)

Publication Number Publication Date
WO2021205780A1 true WO2021205780A1 (ja) 2021-10-14

Family

ID=78023313

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2021/007969 Ceased WO2021205780A1 (ja) 2020-04-10 2021-03-02 高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー

Country Status (4)

Country Link
EP (1) EP4115973A4 (enExample)
JP (2) JP7481151B2 (enExample)
CN (1) CN115379892B (enExample)
WO (1) WO2021205780A1 (enExample)

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP7573817B2 (ja) * 2021-07-30 2024-10-28 ユニ・チャーム株式会社 高吸水性リサイクルポリマー用の2次脱水された高吸水性ポリマーを製造する方法、及び高吸水性リサイクルポリマーを製造する方法

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63241000A (ja) * 1987-03-30 1988-10-06 Mitsubishi Petrochem Co Ltd 含水粉粒体の脱水法
JP2003326161A (ja) 2002-03-06 2003-11-18 Nippon Shokubai Co Ltd 吸水性樹脂の再生方法および吸水剤
JP2006063508A (ja) * 2004-07-30 2006-03-09 Mitsubishi Chemicals Corp 吸水性樹脂複合体およびその製造法並びに吸水性樹脂シートおよび吸水性物品
JP2013520244A (ja) * 2010-02-25 2013-06-06 ザ プロクター アンド ギャンブル カンパニー 超吸収性ポリマー粒子の再利用
WO2013141357A1 (ja) * 2012-03-23 2013-09-26 国立大学法人北海道大学 使用済み高吸水性ポリマーの再生方法

Family Cites Families (12)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102675522B (zh) * 2007-02-05 2014-11-19 株式会社日本触媒 粒子状吸水剂的制造方法
US7910688B2 (en) * 2008-10-22 2011-03-22 Evonik Stockhausen Inc. Recycling superabsorbent polymer fines
JP6333535B2 (ja) * 2013-10-01 2018-05-30 ブイテック株式会社 吸水性樹脂と繊維粉からなる複合物
JP6199243B2 (ja) * 2014-06-12 2017-09-20 ユニ・チャーム株式会社 使用済み衛生用品からリサイクルパルプを製造する方法
CN109563273B (zh) * 2016-06-20 2022-01-11 株式会社日本触媒 吸水剂的制造方法
JP6632494B2 (ja) * 2016-08-05 2020-01-22 ユニ・チャーム株式会社 使用済み吸収性物品からパルプ繊維を回収する方法
JP6913107B2 (ja) * 2016-11-16 2021-08-04 株式会社日本触媒 吸水性樹脂粉末の製造方法及びその製造装置
WO2019124527A1 (ja) * 2017-12-20 2019-06-27 ユニ・チャーム株式会社 リサイクル資材の清浄度の評価方法、リサイクル資材の製造方法、リサイクルパルプ繊維、及びリサイクルパルプ繊維の製造方法
JP7115933B2 (ja) * 2018-02-05 2022-08-09 ユニ・チャーム株式会社 高吸水性ポリマーの再生方法、高吸水性リサイクルポリマーの製造方法、及びアルカリ金属イオン供給源の使用
WO2019151538A1 (ja) * 2018-02-05 2019-08-08 ユニ・チャーム株式会社 高吸水性ポリマーの再生方法、高吸水性リサイクルポリマーの製造方法、及びアルカリ金属イオン供給源の使用
JP7083020B2 (ja) * 2018-05-16 2022-06-09 株式会社日本触媒 吸水性樹脂粉末、及びその製造方法
JP6771633B1 (ja) * 2019-05-30 2020-10-21 ユニ・チャーム株式会社 使用済み吸収性物品由来の高吸水性ポリマーを再生する方法及び使用済み吸収性物品由来のリサイクル高吸水性ポリマー

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63241000A (ja) * 1987-03-30 1988-10-06 Mitsubishi Petrochem Co Ltd 含水粉粒体の脱水法
JP2003326161A (ja) 2002-03-06 2003-11-18 Nippon Shokubai Co Ltd 吸水性樹脂の再生方法および吸水剤
JP2006063508A (ja) * 2004-07-30 2006-03-09 Mitsubishi Chemicals Corp 吸水性樹脂複合体およびその製造法並びに吸水性樹脂シートおよび吸水性物品
JP2013520244A (ja) * 2010-02-25 2013-06-06 ザ プロクター アンド ギャンブル カンパニー 超吸収性ポリマー粒子の再利用
WO2013141357A1 (ja) * 2012-03-23 2013-09-26 国立大学法人北海道大学 使用済み高吸水性ポリマーの再生方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4115973A4

Also Published As

Publication number Publication date
EP4115973A1 (en) 2023-01-11
JP2024096237A (ja) 2024-07-12
JP2021166968A (ja) 2021-10-21
CN115379892B (zh) 2025-11-28
EP4115973A4 (en) 2023-09-13
CN115379892A (zh) 2022-11-22
JP7481151B2 (ja) 2024-05-10
JP7781945B2 (ja) 2025-12-08

Similar Documents

Publication Publication Date Title
RU2368625C2 (ru) Порошкообразный водопоглощающий агент, содержащий водопоглощающую смолу в качестве основного компонента
JP7362886B2 (ja) 吸水性樹脂をリサイクルする方法
EP1265649B1 (en) Permanently wettable superabsorbent fibers
JP6771633B1 (ja) 使用済み吸収性物品由来の高吸水性ポリマーを再生する方法及び使用済み吸収性物品由来のリサイクル高吸水性ポリマー
JP6549841B2 (ja) 吸収性複合体及びその製造方法
CN117729991B (zh) 制造高吸水性再循环聚合物用的经过2次脱水的高吸水性聚合物的方法、以及制造高吸水性再循环聚合物的方法
AU2001247489A1 (en) Permanently wettable superabsorbents fibers
ZA200401195B (en) Superabsorbent polymer.
WO2011090410A1 (en) Absorbent article comprising an absorbent porous foam
KR20170125388A (ko) 수성 액체 흡수성 수지 입자의 제조 방법, 수성 액체 흡수성 수지 입자, 흡수체 및 흡수성 물품
KR102556589B1 (ko) 흡수성 수지 입자 및 그 제조 방법
JP7260334B2 (ja) 吸収体及びその製造方法
JP7781945B2 (ja) 高吸水性リサイクルポリマーの製造方法、及び高吸水性リサイクルポリマー
JP2012506462A (ja) 高吸収性ポリマー微粉を用いた高吸収性ポリマーゲルの生産のためのプロセス
JPWO2017200085A1 (ja) 吸水性樹脂粒子、その製造方法、これを含有してなる吸収体及び吸収性物品
JP7214344B2 (ja) 連続ストランドの高吸水性ポリマーの重合
CN117551286A (zh) 吸水性树脂与其制作方法
WO2023149573A1 (ja) 吸水性樹脂のリサイクル方法、および吸水性樹脂の製造方法
CN100420719C (zh) 吸水性树脂复合体及其组合物
US12357966B2 (en) Superabsorbent polymer and method of producing the same
JP2024095496A (ja) 再生吸水性樹脂の製造方法
JP7605746B2 (ja) カルボキシメチルセルロース粒子の製造方法、前記方法によって製造されたカルボキシメチルセルロース粒子及びそれを含む吸収性物品
JPH02178332A (ja) 吸水性樹脂粉末の帯電防止処理法
JP7291686B2 (ja) 吸水性樹脂粒子及びその製造方法
JP2026092522A (ja) 使用済の、酸基を有する高吸水性ポリマーから再生された高吸水性リサイクルポリマーを製造する方法、高吸水性リサイクルポリマー、及び猫砂

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 21784575

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202217056822

Country of ref document: IN

ENP Entry into the national phase

Ref document number: 2021784575

Country of ref document: EP

Effective date: 20221004

NENP Non-entry into the national phase

Ref country code: DE