WO2020175699A1 - 発泡体シート、及び粘着テープ - Google Patents

発泡体シート、及び粘着テープ Download PDF

Info

Publication number
WO2020175699A1
WO2020175699A1 PCT/JP2020/008518 JP2020008518W WO2020175699A1 WO 2020175699 A1 WO2020175699 A1 WO 2020175699A1 JP 2020008518 W JP2020008518 W JP 2020008518W WO 2020175699 A1 WO2020175699 A1 WO 2020175699A1
Authority
WO
WIPO (PCT)
Prior art keywords
foam sheet
resin
mass
bio
polyolefin resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2020/008518
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
梨絵 松井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to KR1020217026915A priority Critical patent/KR20210135228A/ko
Priority to CN202080016728.7A priority patent/CN113490707A/zh
Priority to JP2020516486A priority patent/JPWO2020175699A1/ja
Publication of WO2020175699A1 publication Critical patent/WO2020175699A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J9/00—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof
    • C08J9/0061—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof characterized by the use of several polymeric components
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F110/00—Homopolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F110/02—Ethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F210/00—Copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F210/02—Ethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J9/00—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof
    • C08J9/04—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof using blowing gases generated by a previously added blowing agent
    • C08J9/06—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof using blowing gases generated by a previously added blowing agent by a chemical blowing agent
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J7/00—Adhesives in the form of films or foils
    • C09J7/20—Adhesives in the form of films or foils characterised by their carriers
    • C09J7/22—Plastics; Metallised plastics
    • C09J7/26—Porous or cellular plastics
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J7/00—Adhesives in the form of films or foils
    • C09J7/30—Adhesives in the form of films or foils characterised by the adhesive composition
    • C09J7/38—Pressure-sensitive adhesives [PSA]
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F2500/00—Characteristics or properties of obtained polyolefins; Use thereof
    • C08F2500/12—Melt flow index or melt flow ratio
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2423/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2423/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment
    • C08J2423/04—Homopolymers or copolymers of ethene
    • C08J2423/06—Polyethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2423/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2423/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment
    • C08J2423/04—Homopolymers or copolymers of ethene
    • C08J2423/08—Copolymers of ethene

Definitions

  • the present invention relates to a foam sheet containing a bio-based polyolefin resin, and an adhesive tape including the foam sheet.
  • a foam sheet obtained by foaming a resin is widely used in various fields such as construction, electronics, and vehicles.
  • Resins derived from petroleum are generally used as the resin used for the foam sheet, but since a large amount of carbon dioxide is emitted during the manufacturing process and the disposal process, environmental load is a problem. Therefore, in order to solve such a problem, studies are being made to use a resin of natural origin.
  • Patent Document 1 polyethylene (bio-based polyethylene) containing a component derived from naturally-occurring ethylene is used, and according to 8 3 1 1/ 1 0 6 8 6 6 (established in 2004) Foams with a measured biomass of 25% or more are described.
  • Patent Document 2 contains a low-density polyethylene resin containing a naturally-derived ethylene component in an amount of 20% by mass or more and 100% by mass or less, a biomass degree of 25% or more, and a gel fraction of 5%. Foams with a content of 60% or less are described.
  • Patent Document 1 Japanese Patent Laid-Open No. 20 1 3 _ 1 5 5 2 25
  • Patent Document 2 JP 2 0 18 _ 6 5 8 9 8 Publication
  • the present inventors have set the bio-rate in the foam sheet to 40% by mass or more, and set the thickness to 0.05 to 1.5. ⁇ 1, expansion ratio 1.5
  • the inventors have found that the above problems can be solved by adjusting the amount by up to 20 times, and have completed the following invention.
  • the present invention relates to the following [1] to [12].
  • a foam sheet having an expansion ratio of 1.5 to 20 times A foam sheet having an expansion ratio of 1.5 to 20 times.
  • the melt index of the polyethylene resin (IV! ⁇ ) is 1.
  • ⁇ _ ⁇ foam sheet according to 1 2 9/1 above is 0 minutes or more [3] or [4].
  • the foam sheet of the present invention is a foam containing at least a bio-based polyolefin resin (8), and has a bio ratio of 40% by mass or more and a thickness of 0.05 to 1.
  • the expansion ratio is 1.5 to 20 times.
  • the foaming ratio of the foam sheet by adjusting the foaming ratio of the foam sheet to 40% by mass or more and adjusting the foaming ratio to a specific range, the foam ratio can be reduced even in a foam sheet having a low environmental load and a small thickness. It is possible to reduce the maximum bubble diameter while keeping the value above a certain level.
  • even a thin foam sheet can be imparted with various performances required for the foam sheet such as impact resistance. ⁇ 02020/175699 4 ⁇ (: 171?2020/008518
  • the foam sheet of the present invention is a foam containing at least a bio-based polyolefin resin (8).
  • the bio-based polyolefin resin () used in the present invention is a polyolefin resin containing a naturally-derived component, and specific examples thereof include a polyethylene-based resin containing naturally-derived ethylene as a constituent unit. More specific examples include homopolymers of naturally-occurring ethylene and copolymers of naturally-occurring ethylene and petroleum-derived olefins. Among these, from the viewpoint of availability, naturally-occurring ethylene and petroleum-derived Copolymers with olefins are preferred.
  • the olefin derived from petroleum is preferably one or more selected from ethylene, propylene, 1-butene, and 1-hexene, and ethylene is particularly preferable.
  • the bio-based polyolefin resin (8) may be an ethylene-vinyl acetate copolymer containing naturally-occurring ethylene as a constituent unit.
  • the bio-based polyolefin resin (eight) may be used alone or in combination of two or more.
  • the content of the structural unit derived from naturally-occurring ethylene is preferably 40 to 98 mass%, more preferably 75 to 97 mass%, 85 to 96 mass% is more preferable. That is, the bio ratio of the bio-based polyolefin resin (8) is preferably 40 to 98% by mass, more preferably 75 to 97% by mass, and further preferably 85 to 96% by mass. ..
  • the content of the structural unit derived from naturally-occurring ethylene is not less than the above lower limit value, the environmental load will be reduced and, for example, the carbon dioxide reduction effect will be enhanced.
  • the content of the structural unit derived from naturally-occurring ethylene is not more than the upper limit value, the crystallization rate will be low when the foamable resin sheet described below is obtained, and therefore the foamable resin sheet having a uniform thickness in the width direction. It is easy to obtain, and various physical properties are likely to be good even if the foam sheet becomes thin.
  • the melt index (IV) of bio-based polyolefin resin (8) is ⁇ 02020/175699 5 ⁇ (: 171?2020/008518
  • the melt index of the bio-based polyolefin resin is 2. ⁇ _ ⁇ more preferably 1 ⁇ 9/1 ⁇ minutes, more preferably from 2.2 to 7.0 9/1 0 min, 2. 4 to 5.09/10 minutes are even more preferable.
  • melt index 8 3 1/1 According to 238, 1 90 ° ⁇ , 2. It is recommended to measure under the conditions.
  • the density of the bio-based polyolefin resin (8) is, for example, ⁇ 900-0.9 409. And preferably from 0.910 to 0.99309. Is.
  • the density of the bio-based polyolefin resin (8) is within the above range, it is easy to improve various performances required for the foam such as impact resistance and flexibility.
  • the bio-based polyolefin resin (8) can be produced by a known method using naturally-derived ethylene and, if necessary, petroleum-derived olefin.
  • the naturally-occurring ethylene which is the raw material for the bio-based polyolefin resin (8), is produced by fermenting the sugar obtained from sugarcane, which is the natural raw material, using the yeast Saccharomyces cerevisiae, which is the fermenting agent, to produce ethanol. , It can be obtained by converting the ethanol into ethylene by catalytic reaction at a temperature over 300° ⁇ using a catalyst such as alumina.
  • the foam sheet may contain a resin other than the bio-based polyolefin resin ().
  • a resin other than the bio-based polyolefin resin for example, it is preferable that the foam sheet contains a polyolefin resin (Mitsumi).
  • Polyolefin resin (Mimi) is a petroleum-based polyolefin resin generally produced from petroleum-derived polyolefin. The use of polyolefin resin (Mitsumi) makes it possible to make the foam sheet thinner. Further, it becomes easy to adjust the compressive strength, the maximum cell diameter and the average cell diameter of the foam sheet within the ranges described below. ⁇ 02020/175699 6 ⁇ (: 171?2020/008518
  • polystyrene resin examples include polyethylene resin, polypropylene resin, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and the like.
  • polyethylene resin ethylene-vinyl acetate At least one selected from copolymers is preferable, and a polyethylene resin is more preferable.
  • the polyolefin resin (Mitsumi) may be used alone or in combination of two or more.
  • polyethylene resins examples include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene compound and a chromium oxide compound, and preferably a polyethylene resin polymerized with a metallocene compound polymerization catalyst is used.
  • a polymerization catalyst such as a Ziegler-Natta compound, a metallocene compound and a chromium oxide compound
  • a polyethylene resin polymerized with a metallocene compound polymerization catalyst is used.
  • the density is 0.93
  • Low-density polyethylene (1_0) which is 3 or less is preferable
  • linear low-density polyethylene (LLDPE) is more preferable.
  • LLDPE linear low-density polyethylene
  • Linear low-density polyethylene is obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more based on the total amount of monomers) and a small amount of ⁇ -olefin, if necessary.
  • the linear low density polyethylene obtained is more preferable.
  • «_ olefins examples include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-year-old cutene. Among them, ⁇ -olefin having 4 to 10 carbon atoms is preferable.
  • the polyethylene resin polymerized by the above-mentioned metallocene compound polymerization catalyst is ⁇ 02020/175699 7 ⁇ (: 171-12020/008518
  • It is preferably linear low-density polyethylene.
  • Polyethylene resin has a density of 0.87 to 0. Is preferred
  • polyethylene resin a plurality of polyethylene resins may be used, and a polyethylene resin having a density outside the above range may be added.
  • the melt index of Poryechiren resin is 1. ⁇ _ ⁇ 1 2 9/1 0 min, 1. More preferably 5-8 9/1 0 minutes, 1.8 to 4.5 More preferably, it is 9/10 minutes.
  • the melt index of the polyethylene resin is within the above range, foaming is appropriately performed, and it becomes easy to reduce the maximum cell diameter of the foam sheet, and the workability and moldability of the foam sheet are improved.
  • the metallocene compound examples include compounds such as bis(cyclopentagenyl) metal complex having a structure in which a transition metal is sandwiched between electronic unsaturated compounds. More specifically, tetravalent transition metals such as titanium, zirconium, nickel, palladium, hafnium, and platinum have one or more cyclopentagenyl rings or their analogs as ligands. Examples of the compound include
  • Such metallocene compounds have uniform active sites and each active site has the same activity.
  • a polymer synthesized using a metallocene compound has high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., and therefore, when a sheet containing a polymer synthesized using a metallocene compound is crosslinked, the crosslinking is Go evenly. As a result, since it can be stretched uniformly, the thickness of the foam sheet is likely to be uniform, and the foam sheet can be easily thinned.
  • Examples of the ligand include a cyclopentaenyl ring, an indenyl ring, and the like. These cyclic compounds may be substituted with a hydrocarbon group, a substituted hydrocarbon group or a hydrocarbon monosubstituted metalloid group. Hydrocarbon group ⁇ 02020/175699 8 ⁇ (: 171?2020/008518
  • Examples thereof include a methyl group, an ethyl group, various propyl groups, various butyl groups, various amyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, Examples thereof include various cetyl groups and phenyl groups.
  • “various” means It means various isomers including 3 ⁇ — t & rt ⁇ 3 ⁇ —.
  • a compound obtained by polymerizing a cyclic compound as an oligomer may be used as a ligand.
  • monovalent anion ligands such as chlorine and bromine or divalent anion chelate ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, arylamides, phosphiides. , Aryl phosphide, etc. may be used.
  • Examples of the metallocene compound containing a tetravalent transition metal or a ligand include cyclopentagenyl titanium tris (dimethyl amide), methyl cyclopenta genenyl titanium tris (dimethyl amide), bis (cyclopentadienyl) titanium di Examples thereof include chloride and dimethylsilyltetramethylcyclopentagenenyl-I-butylamide zirconium dichloride.
  • the metallocene compound when combined with a specific co-catalyst (co-catalyst), exerts an action as a catalyst during the polymerization of various olefins.
  • cocatalysts include methylaluminoxane (1 ⁇ /180) and boron compounds.
  • the ratio of the cocatalyst used to the metallocene compound is preferably 10 to 100,000 mol times, and more preferably 50 to 5,000 mol times.
  • polypropylene resin used as the polyolefin resin examples include polypropylene, propylene-ethylene copolymer containing 50% by mass or more of propylene, and propylene-olefin copolymer containing 50% by mass or more of propylene. Is mentioned. These may be used alone or in combination of two or more.
  • 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene and the like can be mentioned, and among these, carbon number 6 to 12 ⁇ -olefins are preferred.
  • the density of polypropylene resin is from 0.87 to 0. Is preferred, from 890 to ⁇ . Is more preferable, and 0.90 to 0.9.
  • polypropylene resin a plurality of polypropylene resins may be used, and a polypropylene resin having a density outside the above range may be added.
  • the ethylene-vinyl acetate copolymer used as the polyolefin resin (Mitsumi) has, for example, a vinyl acetate content (V 8 amount) of preferably 5 to 40% by mass.
  • the ethylene-vinyl acetate copolymer is more preferably 12 to 35% by mass, further preferably 15 to 30% by mass.
  • the content of vinyl acetate in the ethylene-vinyl acetate copolymer is within the above range, the maximum cell diameter can be reduced, and a foam sheet having excellent flexibility can be obtained.
  • the ethylene-vinyl acetate copolymer used in the present invention may contain, in addition to ethylene and vinyl acetate, vinyl alcohol produced by partially hydrolyzing vinyl acetate.
  • Examples of such an ethylene-vinyl acetate copolymer include “Ultrasen” manufactured by Tosoh Corporation, “Eva Flex” manufactured by Mitsui DuPont Polychemical Co., Ltd., “11 Minami Polyethylene” manufactured by Ube Maruzen Polyethylene Co., Ltd., Asahi. "Suntech” manufactured by Kasei Chemicals Co., Ltd., etc. may be mentioned.
  • the density of the ethylene-vinyl acetate copolymer is from 0.99 to 0.990.89 / ⁇
  • ⁇ . 9 1 0 ⁇ . 9 7 is preferred, ⁇ . 9 1 0 ⁇ . 9 7, more preferably 5 9 / ⁇ 3, ⁇ . 9 2 0 ⁇ .
  • a plurality of ethylene-vinyl acetate copolymers may be used as the ethylene-vinyl acetate copolymer, ⁇ 02020/175699 10 boxes (: 171?2020/008518
  • An ethylene-vinyl acetate copolymer having a density outside the above range may be added.
  • melt index of the ethylene-vinyl acetate copolymer is within the above range, it becomes easy to reduce the maximum cell diameter of the foam sheet, and the foam sheet has good processability and moldability.
  • the content of the bio-based polyolefin resin () in the foam sheet is preferably 42% by mass or more based on the total amount of resin components, from the viewpoint of reducing the load on the environment and increasing the bio ratio of the foam sheet. It is more preferably at least mass%, and even more preferably at least 60 mass%. Further, in order to make the foam sheet thinner and to improve the performance as a foam easily, it is preferable to contain a resin other than the bio-based polyolefin resin (8). From such a viewpoint, the content of the bio-based polyolefin resin (8) is preferably 95% by mass or less, more preferably 85% by mass or less, and further preferably 75% by mass or less.
  • the content of the polyolefin resin (M) is preferably 5% by mass or more, more preferably 15% by mass or more, further preferably 25% by mass or more, based on the total amount of the resin components, and 58% by mass. % Or less, more preferably 50% by mass or less,
  • the content of the polyolefin resin (Mitsumi) above the lower limit value it becomes easier to make the sheet thinner, and the various physical properties required for the foam sheet such as impact resistance, flexibility and mechanical strength are good. It will be easier next time. Further, by setting the content to the upper limit or less, it becomes easy to reduce the environmental load and increase the bio rate of the foam sheet.
  • the polyolefin resin contains a polyethylene resin polymerized with a metallocene compound polymerization catalyst
  • the polyethylene resin is preferably used alone as the polyolefin resin (Mitsumi), but other polyolefin resins You may use together with (B). ⁇ 02020/175699 11 ⁇ (: 171-12020/008518
  • the content of the polyethylene resin polymerized by the polymerization catalyst of the metallocene compound is preferably 40 to 100% by mass, more preferably 50 to 100% by mass, and more preferably 85 to 100% by mass based on the total amount of the polyolefin resin (M). ⁇ 100 mass% is more preferable.
  • the bio-rate of the foam sheet of the present invention is 40% by mass or more. If the bio rate is less than 40% by mass, the load on the environment cannot be reduced. From this viewpoint, the bio-rate is preferably 50% by mass or more, more preferably 60% by mass or more.
  • the upper limit is not particularly limited, but from the viewpoint of strength, flexibility, manufacturing cost of the foam sheet, 90% by mass or less is preferable, 82% by mass or less is more preferable, and 75% by mass or less is More preferably, 68 mass% or less is even more preferable.
  • the bio ratio of the foam sheet can be obtained by multiplying the content ratio of the bio-based polyolefin resin (8) with respect to the total amount of the foam sheet by the viability ratio of the bio-based polyolefin resin (8).
  • the total amount of the foam sheet can be calculated by subtracting the amount of the foaming agent and the components volatilized during the production from the total amount of the resin composition.
  • the bio ratio of the bio-based polyolefin resin (8) is the biomass degree measured by the measurement method specified in 8 3-1 1 ⁇ 1 0 6 8 6 6.
  • the foam sheet of the present invention has a thickness of 0.05 to 1.5. Is. Thickness is ⁇ .
  • the foam sheet properties such as mechanical strength and impact resistance of the foam sheet are
  • the thickness of the foam sheet is preferably 1.2 ⁇ ! ⁇ ! or less, more preferably ⁇ 0.9 ⁇ ! ⁇ ! or less.
  • the expansion ratio of the foam sheet of the present invention is 1.5 to 20 times.
  • the foaming ratio of the foam sheet is less than 1.5 times, the bubble ratio becomes low and the performance as a foam body such as flexibility becomes insufficient.
  • the expansion ratio exceeds 20 times the maximum bubble diameter becomes large, and as a result, it becomes difficult to improve various performances of the foam sheet such as impact resistance.
  • the expansion ratio of the foam sheet is preferably 1.8 to 15 times, more preferably 2.5 to 10 times.
  • the expansion ratio refers to the value calculated by measuring the specific volume before and after foaming (unit: ⁇ /9) and calculating the specific volume after foaming/specific volume before foaming.
  • the maximum cell diameter of the foam sheet of the present invention is preferably 500 or less.
  • the maximum cell diameter of the foam sheet is more preferably 380 or less, and further preferably 300 or less.
  • the maximum cell diameter of the foam sheet is preferably 50 or more, more preferably 80 or more, and further preferably 100 or more.
  • the foam sheet of the present invention has an average cell diameter in the IV!
  • the average cell diameter in the IV! 0 direction and the mouth direction are both preferably 30 to 250, more preferably 50 to 200, and further preferably 60 to 140.
  • the average cell diameter in the 0 direction of the foam sheet is preferably 5 to 250, and more preferably 10 to 140, from the viewpoint of ensuring impact resistance and shock absorption. More preferably, 15 to 100 Mm is more preferable, 20 to 60 Mm is still more preferable.
  • the average bubble diameter is measured according to the following procedure.
  • a foam sheet cut into a 5 Omm square was prepared as a foam sheet sample for measurement. After immersing this in liquid nitrogen for 1 minute, it was cut in the thickness direction along the MD and TD directions with a razor blade. This cross section was taken with a digital microscope ("VHX-900" manufactured by KEYENCE CORPORATION) at a magnification of 200 times, and it exists on the cut surface of 2 mm length in each of MD direction and TD direction. The bubble diameters of all the bubbles were measured, and the procedure was repeated 5 times. Then, the average value of all bubbles was taken as the average bubble diameter in the MD direction and the T D direction. The bubble diameter in the ZD direction was also measured for all the measured bubbles, and the average value was taken as the average bubble diameter in the ZD direction. Further, the maximum value among all the measured bubble diameters was defined as the maximum bubble diameter.
  • MD Machine Direction and means a direction that coincides with the extrusion direction of the foam sheet or the like.
  • TD means a Transverse Direction and means a direction orthogonal to MD and parallel to the foam sheet.
  • ZD means Thickness Direction, which is a direction perpendicular to both 1 ⁇ /10 and Ding 0.
  • the ratio of the average bubble diameter in the MD and TD directions to the average bubble diameter in the ZD direction (hereinafter also referred to as “(MD + TD)/2 ZD”) is preferably 1.3 to 10 and 1.8 to 9 Is more preferable, 2 to 8 is still more preferable, and 2.5 to 6 is still more preferable.
  • the ratio of the average bubble diameter in the MD and T D directions is the average value of the average bubble diameter in the MD direction and the average bubble diameter in the T D direction.
  • the value of 20 can be adjusted by stretching the foam sheet at the time of manufacturing the foam sheet while adjusting the foaming ratio within the above range.
  • the 25% compressive strength of the foam sheet is, for example, 3501 ⁇ 3 or less, but from the viewpoint of flexibility, it is preferably 20001 ⁇ 3 or less, more preferably 1601 ⁇ 3 or less. , 1001 ⁇ 3 or less is more preferable. Further, from the viewpoint of improving flexibility, impact resistance and mechanical strength, the foam sheet preferably has a 25% compressive strength of 20 ⁇ 9 a or more, and 3 51 ⁇ A value of 3 or more is more preferable, and a value of 4 01 ⁇ 3 or more is even more preferable.
  • the 25% compressive strength can be adjusted by the type of resin, cell diameter, expansion ratio, etc. For example, if the expansion ratio is increased, the 25% compression strength value can be decreased.
  • the 25% compressive strength refers to the value obtained by measuring the foam sheet in accordance with “3 ⁇ 6 7 6 7.
  • the foam sheet is preferably crosslinked.
  • the cross-linking degree of the foam sheet is preferably 15% by mass or more.
  • the degree of cross-linking is not less than the above lower limit, it becomes easy to adjust the average cell diameter within the above range, and it becomes easy to make the cells of the foam sheet fine.
  • the degree of crosslinking of the foam sheet is more preferably 25% by mass or more, and further preferably 30% by mass or more.
  • the degree of crosslinking is preferably 65% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less, from the viewpoint of improving the flexibility, impact resistance, impact absorption and the like of the foam sheet. Is more preferable.
  • the foam sheet is obtained by foaming a resin composition containing the above resin and a foaming agent. Further, the foam sheet may be further blended with an additive. Therefore, the foam sheet may be one obtained by foaming a resin composition containing an additive in addition to the resin and the foaming agent.
  • a thermal decomposition type foaming agent is preferable as the foaming agent.
  • Specific examples of the pyrolytic foaming agent include organic or inorganic chemical foaming agents having a decomposition temperature of about 140° to 270°.
  • Organic foaming agents include azodicarbonamide, azodicarboxylic acid metal salts (barium azodicarboxylate, etc.), azo compounds such as azobisisoptyronitrile, 1 ⁇ 1, 1 ⁇ 1'-dinitrosopentamethylene.
  • azo compounds such as azobisisoptyronitrile, 1 ⁇ 1, 1 ⁇ 1'-dinitrosopentamethylene.
  • examples thereof include nitroso compounds such as tetramine, hydrazodicarbonamide, hydrazine derivatives such as 4,4′-oxybis(benzenesulfonyl hydrazide) and toluenesulfonyl hydrazide, and semicarbazide compounds such as toluenesulfonyl semicarbazide.
  • the inorganic foaming agent include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, anhydrous monoso
  • azo compounds and nitroso compounds are preferable from the viewpoint of obtaining fine bubbles, and from the viewpoints of economy and safety, and azodicarbonamide, azobisisobutyronitrile, 1 ⁇ ], 1 ⁇ 1'- Dinitrosopentamethylenetetramine is more preferred, and azodicarbonamide is especially preferred.
  • thermal decomposition type foaming agents can be used alone or in combination of two or more.
  • the blending amount of the thermal decomposition type foaming agent is preferably 1 to 30 parts by mass with respect to 100 parts by mass of the resin component. By using such a blending amount, it is possible to appropriately foam the bubbles of the sheet without bursting. Further, if the blending amount of the thermal decomposition type foaming agent is increased, the foaming ratio becomes high and the flexibility can be improved. Therefore, the content of the thermal decomposition type foaming agent is more preferably 3 to 25 parts by mass, further preferably 5 to 18 parts by mass.
  • the foam sheet preferably contains a cell nucleus control agent as an additive.
  • the cell nucleus modifier include zinc compounds such as zinc oxide and zinc stearate, and organic compounds such as citric acid and urea. Among these, zinc oxide and zinc stearate are more preferable, and only one of them may be used, or both of them may be used. ⁇ 02020/175699 16 ⁇ (: 171?2020/008518
  • the cell nucleus control agent in addition to the foaming agent, it becomes easy to reduce the average cell diameter and the variation in cell diameter.
  • the blending amount of the cell nucleus modifier is preferably 0.1 to 8 parts by mass, more preferably 0.2 to 5 parts by mass, and further preferably 0.3 to 2 parts by mass with respect to 100 parts by mass of the resin component. 5 parts by mass.
  • An antioxidant may be added to the foam sheet as an additive.
  • the antioxidant include phosphorus-based antioxidants, phenol-based antioxidants, sulfur-based antioxidants, amine-based antioxidants and the like.
  • the antioxidant is blended in an amount of 0.01 to 5 parts by mass with respect to 100 parts by mass of the resin component.
  • the foam sheet may contain a colorant as an additive.
  • the colorant is blended to adjust the color of the foam sheet.
  • Specific examples of the colorant include pigments and dyes.
  • the coloring agent is blended in an amount of 0.5 to 5 parts by mass with respect to 100 parts by mass of the resin component.
  • additives that are commonly used in foam sheets such as heat stabilizers, flame retardants, antistatic agents, and fillers, are added to the foam sheet, if necessary. May be.
  • the foam sheet is prepared by blending a resin, a foaming agent and, if necessary, other additives, and kneading the resin composition to form a sheet into a foamable resin sheet, and then ionizing radiation. After cross-linking by a method such as heating, it is preferable to manufacture by a method of heating and foaming in a heating device such as a heating furnace or an oven.
  • the above-mentioned expandable resin sheet is obtained by, for example, kneading various components using a kneading machine such as a Banbury mixer or a pressure kneader to obtain a resin composition, and using an extruder, a calender, a conveyor belt carrier. It may be obtained by continuously extruding by sting or the like.
  • Examples of the cross-linking method of the foamable resin sheet include cross-linking with ionizing radiation and cross-linking with organic peroxide, and cross-linking with ionizing radiation is preferable. ⁇ 02020/175699 17 ⁇ (: 171?2020/008518
  • examples of the ionizing radiation include ultraviolet light, electron beams, electron beams and the like.
  • the irradiation dose of ionizing radiation is preferably 0.5 to 10 IV! "3, more preferably 1.5 to 8 IV! "3.
  • the diameter is small and uniform. It is possible to obtain a foam sheet having a cell diameter.
  • examples of the organic peroxide include diisopropylbenzene hydroperoxide, 2,4-dichlorobenzoylperoxide, benzoylperoxide, and _butylperoxide.
  • the amount of the organic peroxide to be blended is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 7 parts by mass with respect to 100 parts by mass of the resin component.
  • a method for foaming the expandable resin sheet a batch method such as an oven or a continuous foaming method in which the expandable resin sheet is formed into a long sheet shape and continuously passed through a heating furnace is exemplified.
  • the heating temperature is preferably 200 to 320°, more preferably 250 to 300°.
  • the foamable resin sheet is used when foaming.
  • Direction and D-direction at least
  • the foamable resin sheet is It may be stretched in at least one of the unidirectional direction and the unidirectional direction, preferably in both of these directions.
  • the foamable resin sheet may be continuously stretched without being cooled after the foaming while maintaining the molten state at the time of foaming. It may be stretched in a softened state.
  • the foam sheet of the present invention is suitably used for electronic equipment applications. That is, the foam sheet of the present invention is, for example, a mobile phone such as a smartphone, a camera, a game machine, an electronic organizer, a tablet terminal, an electronic device such as a notebook personal computer, preferably a mobile phone such as a smartphone. It is preferably used inside.
  • Foam sheets are used inside electronic devices, for example, as sealants, shock absorbers, and the like.
  • the foam sheet of the present invention may be used for an adhesive tape having the foam sheet as a base material.
  • the adhesive tape comprises, for example, a foam sheet and an adhesive material provided on at least one surface of the foam sheet.
  • the adhesive tape can be adhered to other members via the adhesive material.
  • the adhesive tape may have an adhesive material provided on both sides of the foam sheet, or may have an adhesive material provided on one surface.
  • the pressure-sensitive adhesive is a member having pressure-sensitive adhesiveness, and may be any member that has at least a pressure-sensitive adhesive layer, and may be a single pressure-sensitive adhesive layer laminated on the surface of the foam sheet.
  • a double-sided pressure-sensitive adhesive sheet attached to the surface of the foam sheet may be used, but the pressure-sensitive adhesive layer alone is preferable.
  • the double-sided pressure-sensitive adhesive sheet includes a base material and a pressure-sensitive adhesive layer provided on both surfaces of the base material. The double-sided adhesive sheet is used to bond one adhesive layer to the foam sheet and the other adhesive layer to another member.
  • the pressure-sensitive adhesive forming the pressure-sensitive adhesive layer is not particularly limited, and for example, an acrylic pressure-sensitive adhesive, a urethane pressure-sensitive adhesive, a rubber pressure-sensitive adhesive or the like can be used. Further, a release sheet such as release paper may be attached on the adhesive material.
  • the thickness of the adhesive material is preferably 5 to 200, more preferably 7 to 150, and further preferably 10 to 100.
  • the composition shown in Table 2 was supplied to an extruder and melt-kneaded at 130 ° C to obtain a resin composition.
  • the resin composition was extruded to obtain a long foamable resin sheet.
  • the resin sheet was crosslinked by irradiating both sides of the above long-sized foamable resin sheet with an electron beam having an accelerating voltage of 500 V for 4.5 IV! " 3.
  • the crosslinked foamable resin sheet was crosslinked. It is continuously fed into the foaming furnace held at 250 ° ° by hot air and infrared heater, Then, foaming was performed to obtain a foam sheet having the thickness described in Table 1.
  • Example 2 Each component supplied to the extruder was adjusted as shown in Table 2, and a resin composition was obtained in the same manner as in Example 1. After that, adjust the electron beam irradiation dose so that the degree of cross-linking is as shown in Table 2, and Example 2 was performed in the same manner as in Example 1 except that the degree of stretching was adjusted so that the value of (*)/20 was as described in Table 2.
  • Cross-linking degree (mass %) (Min/Hachi) X 100
  • the average cell diameter and the maximum cell diameter of the foam sheet were measured by the method described in the specification.
  • the foam sheets of each Example have a high bio-rate and a small thickness, but can reduce the maximum cell diameter, and various performances such as impact resistance. Can be understood to be good.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • General Chemical & Material Sciences (AREA)
  • Manufacture Of Porous Articles, And Recovery And Treatment Of Waste Products (AREA)
  • Adhesive Tapes (AREA)
PCT/JP2020/008518 2019-02-28 2020-02-28 発泡体シート、及び粘着テープ Ceased WO2020175699A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
KR1020217026915A KR20210135228A (ko) 2019-02-28 2020-02-28 발포체 시트, 및 점착 테이프
CN202080016728.7A CN113490707A (zh) 2019-02-28 2020-02-28 发泡体片及粘合带
JP2020516486A JPWO2020175699A1 (ja) 2019-02-28 2020-02-28 発泡体シート、及び粘着テープ

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2019-035550 2019-02-28
JP2019035550 2019-02-28

Publications (1)

Publication Number Publication Date
WO2020175699A1 true WO2020175699A1 (ja) 2020-09-03

Family

ID=72239822

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2020/008518 Ceased WO2020175699A1 (ja) 2019-02-28 2020-02-28 発泡体シート、及び粘着テープ

Country Status (4)

Country Link
JP (1) JPWO2020175699A1 (cg-RX-API-DMAC10.html)
KR (1) KR20210135228A (cg-RX-API-DMAC10.html)
CN (1) CN113490707A (cg-RX-API-DMAC10.html)
WO (1) WO2020175699A1 (cg-RX-API-DMAC10.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2023058079A (ja) * 2021-10-13 2023-04-25 三井化学東セロ株式会社 ポリエチレン系樹脂発泡シートおよびパッキン

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013060528A (ja) * 2011-09-13 2013-04-04 Sekisui Plastics Co Ltd ポリエチレン系樹脂発泡シート、発泡成形体、及びポリエチレン系樹脂発泡シートの製造方法
JP2018065898A (ja) * 2016-10-18 2018-04-26 東レ株式会社 発泡体
WO2018181486A1 (ja) * 2017-03-30 2018-10-04 積水化学工業株式会社 樹脂発泡シート、樹脂発泡シートの製造方法、及び粘着テープ

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US7265160B2 (en) * 2001-11-29 2007-09-04 Toray Industries, Inc. Crosslinked biodegradable resin continuous foamed sheet and method for production thereof
JP5919841B2 (ja) 2012-01-27 2016-05-18 東レ株式会社 発泡体
JP6625032B2 (ja) * 2016-09-30 2019-12-25 積水化学工業株式会社 独立気泡樹脂発泡体及びその製造方法

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013060528A (ja) * 2011-09-13 2013-04-04 Sekisui Plastics Co Ltd ポリエチレン系樹脂発泡シート、発泡成形体、及びポリエチレン系樹脂発泡シートの製造方法
JP2018065898A (ja) * 2016-10-18 2018-04-26 東レ株式会社 発泡体
WO2018181486A1 (ja) * 2017-03-30 2018-10-04 積水化学工業株式会社 樹脂発泡シート、樹脂発泡シートの製造方法、及び粘着テープ

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2023058079A (ja) * 2021-10-13 2023-04-25 三井化学東セロ株式会社 ポリエチレン系樹脂発泡シートおよびパッキン

Also Published As

Publication number Publication date
CN113490707A (zh) 2021-10-08
KR20210135228A (ko) 2021-11-12
JPWO2020175699A1 (ja) 2021-12-23

Similar Documents

Publication Publication Date Title
JP6207009B2 (ja) 架橋ポリオレフィン樹脂発泡シート
KR102057636B1 (ko) 가교 폴리올레핀계 수지 발포 시트
US10125201B2 (en) Polyolefin resin foam sheet and adhesive tape
US11046871B2 (en) Polyolefin resin foam sheet and adhesive tape
KR20170063630A (ko) 폴리올레핀계 수지 발포 시트 및 점착 테이프
JP2019137795A (ja) 発泡シート、及び粘着テープ
JP7295623B2 (ja) ポリオレフィン系樹脂発泡シート及びそれを用いた粘着テープ
JP6665340B2 (ja) ポリオレフィン系樹脂発泡シート及び粘着テープ
EP3357958B1 (en) Polyolefin resin foamed sheet and adhesive tape
JP2021031608A (ja) 発泡体シート、及び粘着テープ
JP2018172643A (ja) 発泡シート、及び粘着テープ
JP6625032B2 (ja) 独立気泡樹脂発泡体及びその製造方法
JP2021152099A (ja) 発泡体シート及び粘着テープ
KR102597457B1 (ko) 폴리올레핀계 발포 시트, 그 제조 방법 및 점착 테이프
JP6901476B2 (ja) 架橋樹脂発泡シート、その製造方法、及び粘着テープ
JPWO2020175699A1 (ja) 発泡体シート、及び粘着テープ
JP6918701B2 (ja) ポリオレフィン系発泡シート、その製造方法及び粘着テープ
JP2019065191A (ja) 樹脂発泡シート、樹脂発泡シートの製造方法、及び粘着テープ
JP6956163B2 (ja) 独立気泡樹脂発泡体及びその製造方法
JP7492315B2 (ja) 樹脂発泡シート
JP6898109B2 (ja) 樹脂発泡シート及びその製造方法

Legal Events

Date Code Title Description
ENP Entry into the national phase

Ref document number: 2020516486

Country of ref document: JP

Kind code of ref document: A

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 20762628

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 20762628

Country of ref document: EP

Kind code of ref document: A1