WO2020121799A1 - 熱電池 - Google Patents
熱電池 Download PDFInfo
- Publication number
- WO2020121799A1 WO2020121799A1 PCT/JP2019/046096 JP2019046096W WO2020121799A1 WO 2020121799 A1 WO2020121799 A1 WO 2020121799A1 JP 2019046096 W JP2019046096 W JP 2019046096W WO 2020121799 A1 WO2020121799 A1 WO 2020121799A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- temperature
- electrode
- phase transition
- structural phase
- redox potential
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10N15/00—Thermoelectric devices without a junction of dissimilar materials; Thermomagnetic devices, e.g. using the Nernst-Ettingshausen effect
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10N99/00—Subject matter not provided for in other groups of this subclass
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
- Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y02E60/00—Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
- Y02E60/10—Energy storage using batteries
Definitions
- the present invention relates to a thermal battery that generates electric power due to a temperature change.
- Unused industrial waste heat in Japan is more than twice the amount of electricity used in Japan.
- the amount of solar thermal energy that reaches Japan is 1000 times or more the amount of electric power used in Japan. If a part of these heat energy can be converted into electric energy, consumption of fossil energy can be suppressed and it can contribute to the reduction of carbon dioxide. Further, since the human body also radiates heat energy, if this heat energy can be converted into electric energy, charging of the mobile device becomes unnecessary.
- a "thermoelectric power generation system" capable of inexpensively converting thermal energy near room temperature into electric energy is required.
- thermoelectric generator As a technique for converting a temperature difference into electric energy, for example, a thermoelectric generator using the Seebeck coefficient of a semiconductor is known.
- a thermoelectric generator using the Seebeck coefficient of a semiconductor is known.
- a material (Bi 2 Te 3 ) having high performance near room temperature is used.
- this material has a problem that it is expensive and contains toxic elements. Further, this thermoelectric generator is bulky because of the temperature gradient.
- Patent Document 1 discloses a thermoelectric generator that generates electromotive force by bringing electrodes having different thermoelectromotive forces into contact with the same electrolyte layer and changing the temperature of the entire device. Thermoelectric power generation using the method described in Patent Document 1 has been demonstrated at the basic research level.
- Non-Patent Document 1 the positive electrode is Na 1.6 Co[Fe(CN) 6 ] 0.9 , the negative electrode is Na 0.84 Co[Fe(CM) 6 ] 0.71 , and the electrolytic solution is 10 mol/L.
- a thermoelectric power generation device was prepared using the above NaClO 4 aqueous solution. With this thermoelectric generator, an electromotive force of 24 mV was obtained between 23°C and 50°C. The thermal efficiency of this thermoelectric generator was 1.0%. This value has a Carnot efficiency of 11%.
- Non-Patent Document 2 the positive electrode is Na 1.6 Co[Fe(CN) 6 ] 0.9 , the negative electrode is Na 1.32 Mn[Fe(CM) 6 ] 0.83 , and the electrolytic solution is 10 mol/L.
- the heat generating element was NaClO 4 in propylene carbonate solution of was prepared. With this thermoelectric generator, an electromotive force of 39 mV was obtained between 13°C and 40°C. The thermal efficiency of this thermoelectric generator was 2.3%. This value has a Carnot efficiency of 23%.
- thermoelectromotive force coefficient of Na 1.6 Co[Fe(CN) 6 ] 0.9 is 1.3 mV/K
- thermoelectromotive force coefficient of Na 0.84 Co[Fe(CM) 6 ] 0.71 is 0.
- the thermoelectromotive force coefficient of 5 mV/K, Na 1.32 Mn[Fe(CM) 6 ] 0.83 is ⁇ 0.3 mV/K. In order to obtain higher thermoelectromotive force and thermal efficiency, it is essential to create materials that exhibit higher thermoelectromotive force coefficient.
- thermoelectromotive force generated by the thermoelectric generator is given by the product of the difference between the thermoelectromotive force coefficients of the positive and negative electrode materials and the temperature change. Furthermore, the thermal efficiency of the thermoelectric generator is proportional to the thermoelectromotive force. Therefore, in order to obtain a larger thermoelectromotive force and thermal efficiency, an electrode material having a larger thermoelectromotive force coefficient, an element including the same, and a thermal battery structure including the same have been desired.
- the present invention has been made in view of the above circumstances, and an object of the present invention is to provide a thermal battery that can obtain a larger thermoelectromotive force.
- the thermal battery of this embodiment includes the following modes of implementation.
- An element including a first electrode, a second electrode having a temperature coefficient of redox potential different from that of the first electrode, and an electrolyte is provided, and the first electrode or the second electrode is provided.
- Either or both of the electrodes include a material that undergoes a structural phase transition and a redox potential changes with a change in temperature, and the first electrode and the second electrode are provided in contact with the electrolyte, respectively.
- increasing or decreasing the temperature of the element causes a difference in redox potential between the first electrode and the second electrode to obtain electric power from the element. battery.
- the element is adjusted to a high temperature equal to or higher than the upper critical temperature of the structural phase transition to cause a difference in the redox potential, the temperature of the element is maintained at the high temperature, and electric power is obtained from the element. Or, the element is adjusted to a low temperature below the lower critical temperature of the structural phase transition to cause a difference in the redox potential, and the temperature of the element is maintained at the low temperature,
- the device is adjusted to a high temperature equal to or higher than the upper critical temperature of the structural phase transition to cause a difference in the redox potential, and then the temperature of the device is set to the upper critical temperature and the structural phase transition.
- the device is configured to obtain electric power from the device while being kept at a working temperature between the lower critical temperature, or the device is adjusted to a low temperature below the lower critical temperature of the structural phase transition, and the redox potential is adjusted. And the temperature of the device is maintained at the working temperature to obtain electric power from the device.
- thermoelectric generator in which a first electrode and a second electrode face each other via a single electrolyte, wherein the first electrode undergoes a structural phase transition with an increase in temperature
- the second electrode includes a material A having a large change in electromotive force, the second electrode undergoes a structural phase transition with a rise in temperature, and a material B having a change in electromotive force in the opposite direction to the material A or a rise in temperature.
- a material C that does not undergo structural phase transition and whose electromotive force changes in a direction opposite to that of the material A is used, and the material A is Na x Co 1-y A z [Fe(CN) 6 ] z (however, , A is at least one selected from the group consisting of Fe, Mn, Ni and Zn, 0.8 ⁇ x ⁇ 2.0, 0.0 ⁇ y ⁇ 1.0, 0.7 ⁇ z ⁇ 1.0.
- thermoelectric generator comprising a compound represented by [2A]
- the material C is a compound represented by Na x Co 1-y [Fe(CN) 6 ] z (0.8 ⁇ x ⁇ 2.0, 0.8 ⁇ z ⁇ 1.0) [3A]
- the unit including the first electrode, the second electrode, and the electrolyte is the first electrode of one unit and the second electrode of the other unit.
- thermoelectric generation of the thermal battery of this embodiment It is a sectional view of a thermoelectric generator in one embodiment of the present invention.
- FIG. 6 is a diagram showing a change in electrode capacitance when the NCF film A or NCF90 film A is oxidized in a reference experimental example. It is a schematic diagram of the thermoelectromotive force measuring device used in the reference experiment example. It is a figure which shows the result of having measured the electromotive force of the electrochemical cell in a reference experiment example. It is a figure which shows the change of the capacity of an electrochemical cell in a reference experiment example.
- the thermal battery of this embodiment has an element including a first electrode, a second electrode, and an electrolyte layer.
- the first electrode and the second electrode have different values of the temperature coefficient of the redox potential. Having different values of the temperature coefficient of the redox potential between the first electrode and the second electrode means that when the temperature of each electrode is changed under the same conditions, the redox potential changes and the values are different. It means that. For example, there is a case where one changes a large redox potential and the other changes a small redox potential when the same temperature is changed. Further, when the first electrode and the second electrode are changed to the same temperature T 1 , the redox potentials of positive and negative are reversed (for example, the first electrode is negative redox). It is further preferred that the change in electric potential occurs and the second electrode causes a change in positive redox potential).
- Either or both of the first electrode and the second electrode contain a material that undergoes a structural phase transition and a redox potential changes with a change in temperature.
- Structural phase transition means a change in physical property, such as a change in volume. What kind of structural phase transition occurs due to a change in temperature is, for example, a cooperative behavior between two transition metals.
- the structural phase transition induced by charge transfer and the order-disorder induced structural phase transition of Na are mentioned.
- the change in temperature refers to an increase or decrease in temperature.
- the structural phase transition accompanied by an increase in temperature means that when the upper critical temperature of the structural phase transition of the material is higher than a certain temperature (for example, room temperature), the temperature is increased from the certain temperature to the upper critical temperature or more. In that case, structural phase transition occurs.
- a certain temperature for example, room temperature
- the temperature of a compound that has undergone a structural phase transition due to an increase in temperature is lowered below the lower critical temperature, it returns to the state before the structural phase transition (that is, the temperature The structural phase transition to another state with the fall of) also occurs.
- the compound having a structural phase transition of the present embodiment preferably undergoes a structural phase transition within a range of approximately 20 to 30° C. with approximately room temperature sandwiched therebetween. More specifically, it is preferable that the structural phase transition occurs in any of the range of 0 to 60° C., preferably 10 to 50° C. Both the upper critical temperature and the lower critical temperature are preferably in the range of 0 to 60°C.
- the change in the redox potential means, more specifically, that the redox potential of the material changes by 100 mV or more when the temperature is changed by 30° C. with the critical temperature of the structural phase transition interposed. At this time, it is particularly preferable that the redox potential changes by 150 mV or more.
- the absolute value of the thermoelectromotive force coefficient is preferably 3.3 mV/K or more, particularly preferably 5.0 mV/K or more.
- the material that does not cause structural phase transition in the prior art has, for example, an absolute value of the thermoelectromotive force coefficient of 0.3 to 1.0 mV/K and the like, and the material of the present embodiment has a large potential change compared with these materials. ..
- the material of this embodiment has a thermoelectromotive force constant at a certain temperature that is 3 times or more, preferably 5 times or more that of a material that does not cause a structural phase transition.
- a compound capable of causing the above structural phase transition can be selected from the compounds conventionally used for electrodes.
- Co-PBA cobalt Prussian blue type complex
- A is at least one selected from the group consisting of Fe, Mn, Ni and Zn, The compound represented by 0.8 ⁇ x ⁇ 2.0, 0.0 ⁇ y ⁇ 1.0, 0.7 ⁇ z ⁇ 1.0
- a compound that causes the structural phase transition it is also preferable to use a compound that causes the structural phase transition and is capable of redox.
- a compound that causes the structural phase transition examples include the above-mentioned Co-PBA, a layered oxide (Na x MO 2 , Li x MO 2 :M is a transition metal), a polyanion material (LiFe 1-z M z PO 4 , LiFe 1-z M z SiO 4 ; M is a transition metal) can be used.
- the Co-PBA and the polyanion undergo a structural phase transition induced by cooperative charge transfer between two kinds of transition metals, and the layered oxide is an ordered-disordered structural phase of Na. Cause metastasis.
- the material in which the redox potential changes due to a structural phase transition with a change in temperature may be either the first electrode or the second electrode, or both constituent materials.
- one of the first electrode and the second electrode may be a constituent material of the material that undergoes the structural phase transition, and the other may be a constituent material that is not the material of the structural phase transition.
- the redox potential of the electrode whose constituent material is the structural phase transition is largely changed, and the redox potential of the other electrode is small. Becomes large and a large amount of power can be obtained.
- the material can be appropriately selected from materials that can be used for conventional electrodes.
- a layered oxide that does not cause a structural phase transition and a polyanion that does not cause a structural phase transition which are general battery materials, can be used.
- both the first electrode and the second electrode may be made of a material which is a structural phase transition material.
- one of the electrodes may be made of a material that causes a negative change in redox potential due to a rise in temperature
- the other of the electrodes may be made of a material that causes a change in positive redox potential at a rise in temperature. More preferable.
- the difference in redox potential becomes particularly large, and particularly large electric power can be obtained.
- the difference in the redox potential per temperature change of 30° C. was about 30 mV at ⁇ 20° C. (for example, 10 to 50° C.) above and below room temperature, but in the thermal battery of the present invention, 100 mV or more The difference in redox potential is obtained, and the difference in redox potential about three times or more compared with the conventional one is obtained.
- the thermal battery provided with the material that causes the structural phase transition of the present application can be called a so-called tertiary battery because the conventional secondary battery that is charged by electric energy is charged by a temperature change.
- the first electrode and the second electrode are provided in contact with the electrolyte, respectively.
- the contact with the electrolyte includes a mode in which both the first electrode and the second electrode are immersed in the electrolyte.
- the electrolyte can be appropriately selected and used from those which have been conventionally used in batteries.
- a liquid electrolyte is preferably used as the electrolyte.
- the material whose volume changes due to the structural phase transition is used for the electrode, by adopting the mode of immersing the electrode in the liquid electrolyte, the contact between the electrode and the electrolyte is maintained even if the volume of the electrode changes. Therefore, it can be preferably used.
- the liquid electrolyte has a low electric potential, a non-flammable aqueous electrolytic solution having a small electric potential window can be used, which is advantageous in that it is safe.
- an electrolytic solution obtained by dissolving an alkali metal salt in a solvent can be used.
- the alkali metal salt include sodium perchlorate (NaClO 4 ), sodium chloride (NaCl), lithium perchlorate (LiClO 4 ), and the like.
- the solvent include water, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC) and the like.
- the thermal battery of this embodiment may have another structure for obtaining electric power from the element.
- a terminal for discharging from the electrode, such as a lead wire may be provided.
- the thermal battery of the present embodiment may include a casing or the like that houses the elements.
- the temperature of the element is increased or decreased to cause a difference in redox potential between the first electrode and the second electrode, and electric power is obtained from the element. It is composed.
- the temperature of both the first electrode and the second electrode changes, so that the redox potential of A difference in redox potential occurs between the first electrode and the second electrode having different temperature coefficients.
- the temperature of the entire device may be changed by heating or cooling the part of the thermal battery containing the device. It can also be performed, for example, by heating or cooling the entire thermal battery.
- electric power can be taken out from the element. That is, the heat energy due to the change in the temperature of the element or the heat energy depending on the temperature condition in which the element is placed is converted into electric energy.
- electric power may be obtained from the device by the following steps (1) to (4).
- the steps (1) to (4) can be used independently or in any combination. However, as described below, the steps (1) and (2) are performed, or (3) ) Then, it is preferable to obtain the electric power from the device by performing the process of (4).
- a method of obtaining electric power in the process of (1) and then (2) will be described. (1) The element is adjusted to a high temperature equal to or higher than the upper critical temperature of the structural phase transition to cause a difference in redox potential, the element temperature is kept at the high temperature, and electric power is obtained from the element. This process will be described with reference to FIG. 6.
- the thermal battery Before using the thermal battery of the present embodiment, the thermal battery is in the state of the temperature T N before changing the temperature.
- the temperature T N is a temperature close to room temperature (about 20 to 35° C.).
- the upper critical temperature for each sodium component x is shown by a solid line and the lower critical temperature is shown by a broken line. ing.
- the device is adjusted from the temperature T N to a high temperature T U which is higher than or equal to the upper critical temperature in the material having the structural phase transition.
- the upper critical temperature is the critical temperature of the phase transition (when the temperature is raised) when the material undergoes a phase transition from a low temperature to a high temperature.
- the upper critical temperature differs depending on the material, for example, in the present embodiment, a material having an upper critical temperature in the range of 35 to 55° C. is selected, and the high temperature T U can be set to 50 to 55° C. or higher.
- the temperature of the device exceeds the upper critical temperature, the material undergoes a structural phase transition, resulting in a difference in redox potential between the first electrode and the second electrode.
- the temperature of the element is maintained at the above-mentioned high temperature T U. Since the state in which the difference in the redox potential between the first electrode and the second electrode is generated is maintained, electric power can be obtained from the element.
- the device is adjusted to a low temperature not higher than the lower critical temperature of the structural phase transition to generate a redox potential difference, and the device temperature is kept at a low temperature to obtain electric power from the device.
- the device is adjusted from the temperature T N to a low temperature T D that is lower than or equal to the lower critical temperature in the material that undergoes the structural phase transition.
- the lower critical temperature is the critical temperature of the phase transition (when the temperature is lowered) when the material undergoes a phase transition from a high temperature to a low temperature.
- the lower critical temperature differs depending on the material, for example, in the present embodiment, a material having an upper critical temperature in the range of 30 to 10°C is selected, and the low temperature T D can be set to 20 to 0°C or less.
- the temperature of the device falls below the lower critical temperature, the material undergoes a structural phase transition, resulting in a difference in redox potential between the first electrode and the second electrode.
- the temperature of the element is maintained at the low temperature T D described above. Since the state in which the difference in the redox potential between the first electrode and the second electrode is generated is maintained, electric power can be obtained from the element.
- the discharge can be continued by repeating the process of performing (2) after (1).
- a part of the thermal energy flowing from the high temperature heat source in the process (1) to the low temperature heat source in the process (2) is converted into electric energy.
- the device is adjusted to a high temperature equal to or higher than the upper critical temperature of the structural phase transition to cause a difference in redox potential, and then the device temperature is set between the upper critical temperature and the lower critical temperature of the structural phase transition.
- Power is obtained from the device by keeping it at the operating temperature.
- the element is adjusted from the temperature T N to the above-mentioned high temperature T U.
- T N the temperature of the device exceeds the upper critical temperature
- the material undergoes a structural phase transition, resulting in a difference in redox potential between the first electrode and the second electrode.
- the temperature of the device is adjusted to the working temperature T G , which is a temperature between the upper critical temperature and the lower critical temperature described above.
- the operating temperature T G can be arbitrarily selected as long as it is a value that does not exceed the upper critical temperature and does not exceed the lower critical temperature.
- the value exceeding the upper critical temperature and the value exceeding the lower critical temperature is around room temperature, but the operating temperature T G may be room temperature or may be the same as the temperature T N before use. , May be different.
- the use temperature T G is lower than the upper critical temperature of the structural phase transition, but exceeds the lower critical temperature, so that the material having the structural phase transition does not return to the state before the phase transition. Therefore, since the state in which the difference in redox potential between the first electrode and the second electrode is generated is maintained, electric power can be obtained from the element.
- the device is adjusted to a temperature lower than the lower critical temperature of the structural phase transition to cause a difference in redox potential, and then the temperature of the device is adjusted between the upper critical temperature and the lower critical temperature of the structural phase transition. Power is obtained from the device by keeping it at the operating temperature.
- the element is first adjusted from the temperature T N to the above-mentioned low temperature T D. When the temperature of the device falls below the lower critical temperature, the material undergoes a structural phase transition, resulting in a difference in redox potential between the first electrode and the second electrode.
- the temperature of the device is adjusted to the above-mentioned working temperature T G , which is a temperature between the upper critical temperature and the lower critical temperature described above.
- the use temperature T G may be room temperature, may be the same as the temperature T N before use, or may be different.
- the temperature of the element is maintained at the above-mentioned working temperature T G. Since the use temperature T G is higher than the lower critical temperature of the structural phase transition but lower than the upper critical temperature, the material having the structural phase transition does not return to the state before the phase transition. Therefore, since the state in which the difference in redox potential between the first electrode and the second electrode is generated is maintained, electric power can be obtained from the element.
- the discharge can be continued by repeating the process of performing (4) after (3). Thermodynamically, a part of the thermal energy flowing from the high temperature heat source in the process (3) to the low temperature heat source in the process (4) is converted into electric energy.
- FIG. 7 is a cross-sectional view of a thermoelectric generator that is one mode of an element included in the thermoelectric battery of this embodiment.
- the thermoelectric generator 1 of the present embodiment includes a unit 5 having a first electrode 2, a second electrode 3 and an electrolyte 4.
- the first electrode 2 is provided on one surface 6a of the collecting electrode 6, and the second electrode 3 is provided on the other surface 6b of the collecting electrode 6,
- the second electrodes 3 are arranged so as to face each other with the collector electrode 6 interposed therebetween.
- the first electrode 2 and the second electrode 3 are arranged so as to face each other with the separator 7 in between.
- first electrode 2 and the second electrode 3 are arranged so as to face each other with a predetermined gap therebetween, with a single electrolyte 4 impregnated in the separator 7 interposed therebetween.
- the unit 5 having the first electrode 2, the second electrode 3 and the electrolyte 4, the first electrode 2 of one unit 5 and the second electrode 3 of the other unit 5 form the collecting electrode 6.
- a plurality of layers are stacked so as to be adjacent to each other.
- the first electrode 2 and the second electrode 3 are electrically connected via the lead wire 8.
- a circuit (not shown) or a device (not shown) for extracting the current generated in the thermoelectric generator 1 may be provided in the middle of the lead wire 8. Further, these constituent elements are sealed with a laminate film 9.
- the first electrode 2 and the second electrode 3 are preferably insulated to prevent a short circuit.
- insulating means include a gap between the collector electrode 6 and the laminate film 9, and a gap between the electrolyte 4 (separator 7) and the laminate film 9 (the upper and lower ends of the collector electrode 6 and the electrolyte 4 in the figure, respectively).
- an insulating material such as a binder resin described later.
- the first electrode 2 and the second electrode 3 include a material in which the same metal ion reversibly enters and leaves.
- the first electrode 2 and the second electrode 3 may include a material in which the same metal ions are precipitated or alloyed.
- the first electrode 2 contains a material A that undergoes a structural phase transition with a rise in temperature and the electromotive force of which changes greatly
- the second electrode 3 contains an alkali metal B.
- the second electrode 3 undergoes a structural phase transition with an increase in temperature, and a material B whose electromotive force changes in the opposite direction to the material A with an increase in temperature, or a structural phase with an increase in temperature. It includes a material C which does not change and whose electromotive force changes in the opposite direction to the material A with increasing temperature.
- the fact that the electromotive force of the material A significantly changes due to the structural phase transition accompanied by the temperature rise means that the electromotive force greatly changes as the temperature rises as compared with the material which does not show the structural phase transition.
- the material A exhibiting a structural phase transition has an absolute value of thermoelectromotive force coefficient of about 10 mV/K
- the material C exhibiting no structural phase transition has a maximum absolute value of thermoelectromotive force coefficient. Some have 1.3 mV/K.
- the material A was Na x Co 1-y A z [Fe(CN) 6 ] z , Na x Co 1-y A z [Fe(CN) 6 ] z (where A is Fe, Mn, Ni and Zn). At least one selected from the group consisting of 0.8 ⁇ x ⁇ 2.0, 0.0 ⁇ y ⁇ 1.0, 0.7 ⁇ z ⁇ 1.0). Specific examples of such a compound include Na 1.60 Co 0.44 Mn 0.56 [Fe(CN) 6 ] 0.90 .
- the material A is preferably a material that undergoes a structural phase transition at a temperature not higher than the midpoint of the temperature change of the environment in which the thermoelectric generator 1 is used, and that the electromotive force changes greatly.
- the material undergoes a structural phase transition at 30° C. or less and the electromotive force greatly changes.
- the material C may be a material that does not undergo a structural phase transition with an increase in temperature and whose redox potential changes in the opposite direction to the material A with an increase in temperature.
- the first electrode 2 may include a binder resin (binder) or a conductive auxiliary agent in addition to the material A described above.
- binder resin include polyvinylidene fluoride (PVdF) resin, polytetrafluoroethylene (PTFE) resin, and fluororubber.
- PTFE polytetrafluoroethylene
- conductive aid include Ketjen black, acetylene black (AB), furnace black, vapor grown carbon fiber (VGCF), carbon nanotube and the like.
- an electrolytic solution prepared by dissolving an alkali metal salt in a solvent is used.
- the alkali metal salt include sodium perchlorate (NaClO 4 ), sodium chloride (NaCl), lithium perchlorate (LiClO 4 ), and the like.
- the solvent include water, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC) and the like.
- an aqueous electrolyte is preferable, and an aqueous sodium chloride solution is more preferable, because it is inexpensive.
- thermoelectric generator 1 a unit 5 having the first electrode 2, the second electrode 3 and the electrolyte 4 is different from the first electrode 2 of one unit 5 and the unit 5 of the other unit.
- thermoelectric generator 1 of the present embodiment may be composed of one unit 5 having the first electrode 2, the second electrode 3 and the electrolyte 4.
- thermoelectric generator 1 of the present embodiment a larger thermoelectromotive force can be obtained, and it is possible to convert thermal energy into electric energy by utilizing the temperature change of the entire element. Further, by using the water-based electrolyte, it is possible to obtain the thermoelectric power generation element 1 which is less expensive and has less environmental load when discarded.
- the first electrode 2 includes a material A that undergoes a structural phase transition as the temperature rises and the electric potential changes greatly, and the second electrode 3 undergoes a structural phase transition as the temperature rises,
- the material B whose potential changes in the opposite direction to the material A with the increase, or the structural phase transition which does not change with the temperature increase and the potential changes in the opposite direction to the material A with the temperature increase Since it contains the material C that does, the thermoelectric generator 1 can generate electricity in the following manner. A case where the second electrode 3 contains the material B will be described.
- the temperature of the thermoelectric generator 1, that is, the temperature of the first electrode 2 and the temperature of the second electrode 3 are increased by the heat of the human body, the solar heat, the air temperature, or the like.
- the material A contained in the first electrode 2 undergoes a structural phase transition, and the potential of the first electrode 2 greatly changes.
- the material B contained in the second electrode 3 undergoes a structural phase transition, and the potential of the second electrode 3 changes in the direction opposite to that of the first electrode 2.
- a potential difference is generated between the first electrode 2 and the second electrode 3
- an electromotive force is generated between the electrodes due to a change in potential (change in electromotive force)
- the thermoelectric element 1 is charged. ..
- the charged electrical energy can be taken out by discharging.
- the temperature of the thermoelectric generator 1, that is, the temperature of the first electrode 2 and the temperature of the second electrode 3 are decreased by moving away from the human body, cutting off solar heat, lowering the air temperature, and the like.
- the material A contained in the first electrode 2 undergoes a structural phase transition, and the potential of the first electrode 2 largely changes in the direction opposite to that when the temperature rises.
- the material B contained in the second electrode 3 undergoes a structural phase transition, and the potential of the second electrode 3 changes in the direction opposite to that of the first electrode 2.
- a potential difference occurs between the first electrode 2 and the second electrode 3, and the thermoelectric generator 1 is charged.
- the charged electrical energy can be taken out by discharging.
- the second electrode 3 contains the material C.
- the temperature of the thermoelectric generator 1, that is, the temperature of the first electrode 2 and the temperature of the second electrode 3 are increased by the heat of the human body, the solar heat, the air temperature, or the like.
- the material A contained in the first electrode 2 undergoes a structural phase transition, and the potential of the first electrode 2 greatly changes.
- the potential of the second electrode 3 changes in the direction opposite to that of the first electrode 2.
- a potential difference is generated between the first electrode 2 and the second electrode 3, and the thermoelectric generator 1 is charged.
- the charged electrical energy can be taken out by discharging.
- the temperature of the thermoelectric generator 1, that is, the temperature of the first electrode 2 and the temperature of the second electrode 3 are decreased by moving away from the human body, cutting off solar heat, lowering the air temperature, and the like. Then, the material A contained in the first electrode 2 undergoes a structural phase transition, and the potential of the first electrode 2 largely changes in the direction opposite to that when the temperature rises. On the other hand, although the material C contained in the second electrode 3 does not undergo structural phase transition, the potential of the second electrode 3 changes in the direction opposite to that of the first electrode 2. As a result, a potential difference is generated between the first electrode 2 and the second electrode 3, and the thermoelectric generator 1 is charged. The charged electrical energy can be taken out by discharging.
- thermoelectric generator element 1 can be thinned and downsized.
- Indium oxide was prepared by electrolytic deposition using an aqueous solution containing 0.8 mmol/L of K 3 [Fe(CN) 6 ], 0.5 mmol/L of Co(NO 3 ) 2 and 5 mol/L of NaNO 3.
- An NCF90 film was formed on a tin (ITO) electrode plate.
- the voltage was 0.45 V and the voltage application time was 10 minutes.
- an electrode (second electrode) having an electrode layer made of the NCF90 film on the ITO electrode plate was obtained.
- Composition analysis of the NCF film and the NCF90 film formed on the ITO electrode plate by inductively coupled plasma (ICP) emission spectroscopy revealed that the material forming the NCF film was Na x Co[Fe(CN) 6 ] 0.82. It was found that the material forming the NCF90 film was Na 1.6 Co[Fe(CN) 6 ] 0.9 .
- ICP inductively coupled plasma
- the potential for each temperature of the NCF film of the first electrode was measured with the Ag/AgCl standard electrode as the counter electrode.
- An aqueous solution containing 17 mol/kg of sodium perchlorate (NaClO 4 ) was used as the electrolytic solution.
- the graph of FIG. 1 shows a phase diagram of the NCF film in which the vertical axis is T (temperature).
- T temperature
- the hollow circles indicate the critical temperature during temperature increase
- the black circles indicate the critical temperature during temperature decrease.
- the critical temperature at the time of temperature increase is plotted by a solid line
- the critical temperature at a high temperature is plotted by a broken line.
- the graph of FIG. 2 shows a diagram of the NCF film whose vertical axis is a (lattice constant, unit ⁇ ) measured by an X-ray diffractometer.
- the high temperature phase (the part above the solid line in the figure) is a phase containing a large amount of Co 2+ and has a large volume.
- the low temperature phase (the portion below the broken line in the figure) is a phase containing a large amount of Co 3+ and has a small volume.
- the discharge curve of the NCF film is shown in the graph of FIG.
- the vertical axis of the lower graph is V (electromotive force), and the horizontal axis is x, showing the content (concentration) of sodium contained in the NCF film.
- the potential curve at this time is shown by a one-dot chain line. From the results of FIG. 3, in the potential curve when the temperature of the electrolytic solution indicated by the broken line was 10° C., plateaus (the portions where the curves were flat) were observed near 0.95V and 0.5V. At this time, the temperature of the NCF film is also 10°C. Further, in the potential curve shown by the solid line where the temperature of the electrolytic solution is 50° C., the potential of the plateau on the high potential side is reduced, and for example, it is reduced by 150 mV at the 0.2 point on the horizontal axis. It is considered that this is because the temperature of the NCF film also rises (the temperature of the NCF film also reaches 50° C.) as the temperature of the electrolytic solution rises, and the NCF film undergoes a phase transition.
- An electromotive force (difference in redox potential) measurement circuit was connected to the electrode of this battery cell.
- the electromotive force (V cell ) was measured by heating or cooling the battery cell and charging/discharging.
- FIG. 5 A phase diagram of the NCMF film is shown in FIG. 5, where the vertical axis is T (temperature) and the horizontal axis is x (Na content, Na concentration in crystal).
- T temperature
- x Na content, Na concentration in crystal
- the hollow circles indicate the critical temperature during temperature increase
- the black circles indicate the critical temperature during temperature decrease.
- the critical temperature at the time of temperature increase was plotted by a solid line
- the critical temperature at the time of temperature decrease was plotted by a broken line.
- the high temperature phase (the part above the solid line in the figure) is a phase containing a large amount of Co 2+ and has a large volume.
- the low temperature phase (the portion below the broken line in the figure) is a phase containing a large amount of Co 3+ and has a small volume.
- the NCMF film shows that the structural phase transition occurs depending on the temperature for each x (sodium content), and like the NCF film, a potential difference occurs with the temperature change, which indicates that it can be used for a thermal battery.
- Indium oxide was prepared by electrolytic deposition using an aqueous solution containing 0.8 mmol/L of K 3 [Fe(CN) 6 ], 0.5 mmol/L of Co(NO 3 ) 2 and 5 mol/L of NaNO 3.
- the NCF90 film A was formed on the tin (ITO) electrode plate.
- the voltage was 0.45 V and the time for applying the voltage was 10 minutes.
- an electrode (electrode 2A) having an electrode layer made of the NCF90 film on the ITO electrode plate was obtained.
- the material forming the NCF90 film A was Na 1.6 Co[Fe(CN) 6 ] 0. It turned out to be 9 .
- ICP inductively coupled plasma
- a plasma emission spectroscopy analyzer ICP-8100 manufactured by Shimadzu Corporation was used as the inductively coupled plasma (ICP) device.
- the potential curve (discharge curve) of the NCF film of electrode 1A was measured using the Ag/AgCl standard electrode as the counter electrode.
- An aqueous solution containing 17 mol/kg of sodium perchlorate (NaClO 4 ) was used as the electrolytic solution.
- the temperature of the electrolytic solution was set to 18.5° C. and the measurement of the potential curve of the NCF film A was started. The potential curve at this time is shown by the solid line in FIG.
- the temperature of the electrolytic solution was set to 60° C. and the potential curve of the NCF film A was measured. The potential curve at this time is shown by a broken line in FIG.
- the potential curve of the NCF film A was measured by setting the temperature of the electrolytic solution to 18.5°C.
- the potential curve at this time is shown by the alternate long and short dash line in FIG. From the results of FIG. 8, in the potential curve in which the temperature of the electrolytic solution indicated by the solid line and the alternate long and short dash line is 18.5° C., a plateau (a part where the curve is flat) is observed near 0.95 V and 0.5 V. It was At this time, the temperature of the NCF film A is also 18.5°C. Further, in the potential curve in which the temperature of the electrolytic solution is 60° C., which is indicated by the broken line, the potential of the plateau on the high potential side decreases by 200 mV.
- the NCF film A of the electrode 1A was oxidized to 0.97V. At this time, the applied current was 20 ⁇ A. Further, the NCF90 film A of the electrode 2A was oxidized to 1.0V. At this time, the applied current was 16 ⁇ A.
- FIG. 10 shows the change in potential.
- the thermoelectromotive force of the electrode was measured using the electrochemical cell 100 (corresponding to NCF/NCF90 thermal battery) shown in FIG.
- the electrochemical cell 100 includes a first electrode 101 (electrode 1A), a second electrode 102 (electrode 2A), and an electrolyte 103.
- the first electrode 101 and the second electrode 102 are arranged so as to face each other with a predetermined gap therebetween, with a single electrolyte 103 housed in a case 104 interposed therebetween. Further, the first electrode 101 and the second electrode 102 are electrically connected to each other via a lead wire 105. Further, the case 104 is arranged on the heater 106.
- the electrode having the NCF film A was used as the electrode 1A (positive electrode) 101.
- the electrode having the NCF90 film A was used as the electrode 2A (negative electrode) 102.
- An aqueous solution containing 17 mol/kg of sodium perchlorate (NaClO 4 ) was used as the electrolyte 103.
- the thermal battery of the present invention can be used for a thermoelectric generation element that converts industrial waste heat, solar heat, human body heat, etc. into electric energy, a thermoelectric generation system, and the like.
- the thermoelectric generator of the present invention can be used as a stationary thermoelectric generator, a mobile electric generator, a hybrid solar energy generator, and the like.
- SYMBOLS 1... Thermoelectric generator element, 2... 1st electrode (electrode 1A), 3... 2nd electrode (electrode 2A), 4... Electrolyte, 5... Unit, 6... Collection electrode , 7... Separator, 8... Lead wire, 9... Laminated film.
Landscapes
- Hybrid Cells (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2020559069A JP7526483B2 (ja) | 2018-12-14 | 2019-11-26 | 熱電池 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2018234327 | 2018-12-14 | ||
| JP2018-234327 | 2018-12-14 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2020121799A1 true WO2020121799A1 (ja) | 2020-06-18 |
Family
ID=71076343
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2019/046096 Ceased WO2020121799A1 (ja) | 2018-12-14 | 2019-11-26 | 熱電池 |
Country Status (2)
| Country | Link |
|---|---|
| JP (1) | JP7526483B2 (enExample) |
| WO (1) | WO2020121799A1 (enExample) |
Cited By (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2022154776A (ja) * | 2021-03-30 | 2022-10-13 | 国立大学法人 筑波大学 | 三次電池、IoT機器 |
| WO2022239856A1 (ja) * | 2021-05-14 | 2022-11-17 | 国立大学法人東京工業大学 | 熱電変換装置及びコバルト金属錯体 |
| WO2023145579A1 (ja) * | 2022-01-25 | 2023-08-03 | 国立大学法人 筑波大学 | 舗装構造物 |
| JP2024057359A (ja) * | 2022-10-12 | 2024-04-24 | 国立大学法人 筑波大学 | 三次電池用電極、三次電池、三次電池用電極の製造方法 |
| WO2024122505A1 (ja) * | 2022-12-09 | 2024-06-13 | 株式会社アイシン | 熱電発電装置 |
| KR20240171799A (ko) * | 2023-05-31 | 2024-12-09 | 한양대학교 산학협력단 | 열전지 소자 |
| JP7868906B1 (ja) * | 2025-11-05 | 2026-06-02 | 株式会社elleThermo | ラミネート型電池およびラミネート型電池の製造方法 |
Citations (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2011030790A1 (ja) * | 2009-09-09 | 2011-03-17 | 独立行政法人産業技術総合研究所 | 電気化学素子及びその製造方法 |
| JP2016096024A (ja) * | 2014-11-14 | 2016-05-26 | 国立大学法人京都大学 | 二次電池 |
| JP2018073596A (ja) * | 2016-10-28 | 2018-05-10 | 国立大学法人 筑波大学 | 熱発電素子 |
-
2019
- 2019-11-26 JP JP2020559069A patent/JP7526483B2/ja active Active
- 2019-11-26 WO PCT/JP2019/046096 patent/WO2020121799A1/ja not_active Ceased
Patent Citations (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2011030790A1 (ja) * | 2009-09-09 | 2011-03-17 | 独立行政法人産業技術総合研究所 | 電気化学素子及びその製造方法 |
| JP2016096024A (ja) * | 2014-11-14 | 2016-05-26 | 国立大学法人京都大学 | 二次電池 |
| JP2018073596A (ja) * | 2016-10-28 | 2018-05-10 | 国立大学法人 筑波大学 | 熱発電素子 |
Cited By (12)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2022154776A (ja) * | 2021-03-30 | 2022-10-13 | 国立大学法人 筑波大学 | 三次電池、IoT機器 |
| JP7781384B2 (ja) | 2021-03-30 | 2025-12-08 | 国立大学法人 筑波大学 | 三次電池、IoT機器 |
| WO2022239856A1 (ja) * | 2021-05-14 | 2022-11-17 | 国立大学法人東京工業大学 | 熱電変換装置及びコバルト金属錯体 |
| WO2023145579A1 (ja) * | 2022-01-25 | 2023-08-03 | 国立大学法人 筑波大学 | 舗装構造物 |
| JP2023108416A (ja) * | 2022-01-25 | 2023-08-04 | 国立大学法人 筑波大学 | 舗装構造物 |
| JP7919632B2 (ja) | 2022-01-25 | 2026-09-14 | 国立大学法人 筑波大学 | 舗装構造物 |
| JP2024057359A (ja) * | 2022-10-12 | 2024-04-24 | 国立大学法人 筑波大学 | 三次電池用電極、三次電池、三次電池用電極の製造方法 |
| JP7911392B2 (ja) | 2022-10-12 | 2026-08-26 | 国立大学法人 筑波大学 | 三次電池用電極、三次電池、三次電池用電極の製造方法 |
| WO2024122505A1 (ja) * | 2022-12-09 | 2024-06-13 | 株式会社アイシン | 熱電発電装置 |
| KR20240171799A (ko) * | 2023-05-31 | 2024-12-09 | 한양대학교 산학협력단 | 열전지 소자 |
| KR102960448B1 (ko) * | 2023-05-31 | 2026-04-30 | 한양대학교 산학협력단 | 열전지 소자 |
| JP7868906B1 (ja) * | 2025-11-05 | 2026-06-02 | 株式会社elleThermo | ラミネート型電池およびラミネート型電池の製造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7526483B2 (ja) | 2024-08-01 |
| JPWO2020121799A1 (ja) | 2021-11-04 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7526483B2 (ja) | 熱電池 | |
| Lai et al. | A hydrated NH4V3O8 nanobelt electrode for superior aqueous and quasi-solid-state zinc ion batteries | |
| Chodankar et al. | Two‐dimensional materials for high‐energy solid‐state asymmetric pseudocapacitors with high mass loadings | |
| JP6039258B2 (ja) | 高電圧の充電式マグネシウム電池 | |
| KR102182496B1 (ko) | 코발트 옥시하이드록사이드를 포함하는 전기화학 소자 전극 | |
| CN108370011A (zh) | 可充电式铝离子电池 | |
| JP2018530100A (ja) | 水溶媒和ガラス/非晶質固体イオン伝導体 | |
| WO2019181526A1 (ja) | 電気化学キャパシタ | |
| EP3482443B1 (en) | Metal plating-based electrical energy storage cell | |
| JP5378038B2 (ja) | リチウム空気電池 | |
| US20190148763A1 (en) | Self-charging and/or self-cycling electrochemical cells | |
| JPWO2018079325A1 (ja) | 熱化学電池 | |
| JP6908256B2 (ja) | 熱発電素子 | |
| Shan et al. | High purity Mn5O8 nanoparticles with a high overpotential to gas evolution reactions for high voltage aqueous sodium-ion electrochemical storage | |
| JP2009064584A (ja) | 非水電解質電池 | |
| CN111656597A (zh) | 热电电容器 | |
| WO2018013485A1 (en) | Self-charging and/or self-cycling electrochemical cells | |
| Malka et al. | Horizons for modern electrochemistry related to energy storage and conversion, a review | |
| US20220376223A1 (en) | Metallic ion intercalated layered structures | |
| Palmieri et al. | Cobalt doping as a pathway to stabilize the solid-state conversion chemistry of manganese oxide anodes in Li-ion batteries | |
| CN106575758A (zh) | 包含锌离子的可充电电池 | |
| KR20240013152A (ko) | 높은 에너지 밀도를 갖는 에너지 저장 장치를 위한 다가 VOx/그래핀 나노복합체 전극의 용이한 제조 | |
| Onoh et al. | Understanding the chemistry of graphene oxide on redox flow lithium‐ion batteries with a view to enhancing the battery's high‐density storage | |
| KR20130110350A (ko) | 지르코늄이 도핑된 세륨산화물, 그 제조방법, 및 상기 산화물을 촉매로 포함하는 금속공기 2차전지용 공기전극 | |
| JP2014026805A (ja) | 電極材料の製造方法、電池および電極部材 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 19894479 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2020559069 Country of ref document: JP Kind code of ref document: A |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 19894479 Country of ref document: EP Kind code of ref document: A1 |