WO2019186518A1 - Asymmetric composite membranes and modified substrates used in their preparation - Google Patents
Asymmetric composite membranes and modified substrates used in their preparation Download PDFInfo
- Publication number
- WO2019186518A1 WO2019186518A1 PCT/IB2019/052649 IB2019052649W WO2019186518A1 WO 2019186518 A1 WO2019186518 A1 WO 2019186518A1 IB 2019052649 W IB2019052649 W IB 2019052649W WO 2019186518 A1 WO2019186518 A1 WO 2019186518A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- poly
- polyolefin
- sheet
- microporous sheet
- contacted
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D67/00—Processes specially adapted for manufacturing semi-permeable membranes for separation processes or apparatus
- B01D67/0081—After-treatment of organic or inorganic membranes
- B01D67/0093—Chemical modification
- B01D67/00931—Chemical modification by introduction of specific groups after membrane formation, e.g. by grafting
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D67/00—Processes specially adapted for manufacturing semi-permeable membranes for separation processes or apparatus
- B01D67/0081—After-treatment of organic or inorganic membranes
- B01D67/0093—Chemical modification
- B01D67/00933—Chemical modification by addition of a layer chemically bonded to the membrane
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D69/00—Semi-permeable membranes for separation processes or apparatus characterised by their form, structure or properties; Manufacturing processes specially adapted therefor
- B01D69/02—Semi-permeable membranes for separation processes or apparatus characterised by their form, structure or properties; Manufacturing processes specially adapted therefor characterised by their properties
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D69/00—Semi-permeable membranes for separation processes or apparatus characterised by their form, structure or properties; Manufacturing processes specially adapted therefor
- B01D69/12—Composite membranes; Ultra-thin membranes
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/26—Polyalkenes
- B01D71/261—Polyethylene
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/28—Polymers of vinyl aromatic compounds
- B01D71/281—Polystyrene
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/38—Polyalkenylalcohols; Polyalkenylesters; Polyalkenylethers; Polyalkenylaldehydes; Polyalkenylketones; Polyalkenylacetals; Polyalkenylketals
- B01D71/381—Polyvinylalcohol
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/76—Macromolecular material not specifically provided for in a single one of groups B01D71/08 - B01D71/74
- B01D71/82—Macromolecular material not specifically provided for in a single one of groups B01D71/08 - B01D71/74 characterised by the presence of specified groups, e.g. introduced by chemical after-treatment
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/02—Hydrophilization
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/30—Cross-linking
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/38—Graft polymerization
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/38—Graft polymerization
- B01D2323/385—Graft polymerization involving radiation
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/40—Details relating to membrane preparation in-situ membrane formation
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2325/00—Details relating to properties of membranes
- B01D2325/02—Details relating to pores or porosity of the membranes
- B01D2325/022—Asymmetric membranes
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2325/00—Details relating to properties of membranes
- B01D2325/02—Details relating to pores or porosity of the membranes
- B01D2325/022—Asymmetric membranes
- B01D2325/0233—Asymmetric membranes with clearly distinguishable layers
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2325/00—Details relating to properties of membranes
- B01D2325/30—Chemical resistance
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D67/00—Processes specially adapted for manufacturing semi-permeable membranes for separation processes or apparatus
- B01D67/0081—After-treatment of organic or inorganic membranes
- B01D67/0095—Drying
Definitions
- the invention relates to a durable water permeable asymmetric composite membrane with high levels of protein rejection, and substrates for use in their preparation.
- the invention relates to a durable water permeable asymmetric composite membrane consisting of a film of partially cross-linked poly ( ethenol ) adhered to a hydrophilicitized microporous sheet of poly ( ethylene ) .
- the publication of Ogiwara et al (1981) discloses the photografting on poly (propylene ) and low-density poly ( ethylene ) (LDPE) films on which sensitizers were coated beforehand.
- the sensitizers coated on films enabled vinyl monomers, such as methyl methacrylate, acrylic acid and methacrylic acid to graft easily with high yields.
- the hydrophilic monomers acrylic acid and methacrylic acid were conveniently grafted using them in aqueous solution in a liquid phase system.
- Allmer et al (1988) discloses the modification of surfaces of LDPE, high-density poly ( ethylene ) (HDPE) and polystyrene by grafting with acrylic acid. The grafting is performed in the vapor-phase and increased the wettability of the polymer. It was observed that acetone was able to initiate grafting and was found to promote and direct grafting to the surface.
- the later publication of Allmer et al (1989) discloses the grafting of the surface of LDPE with glycidyl acrylate and glycidyl methacrylate by photoinitiation. Acetone and ethanol were used as solvents, with acetone yielding slightly more grafting at the surface.
- the publication of Singleton et al (1993) discloses a method of making a polymeric sheet wettable by aqueous solvents and useful as an electrode separator in an electrochemical device.
- the polymeric sheet is formed from fibres which comprise poly (propylene ) alone and is distinguished from a membrane formed from a microporous polymer sheet.
- Hirooka and Kawazu discloses alkaline separators prepared from unsaturated carboxylic acid grafted poly ( ethylene ) - poly (propylene ) fibre sheets. Again, the sheets used as a substrate in these studies are distinguished from a membrane formed from a microporous polymer sheet.
- the publication of El Kholdi et al (2004) discloses a continuous process for the graft polymerisation of acrylic acid from monomer solutions in water onto LDPE.
- the publication of Bai et al (2011) discloses the preparation of a hot melt adhesive of grafted low-density poly ( ethylene ) (LDPE) .
- the adhesive is prepared by surface UV photografting of acrylic acid onto the LDPE with benzophenone as the photoinitiator.
- the publication of Choi discloses a method for producing an acrylic graft polymer on the surface of a polyolefin article comprising the steps of immersing the article in a solution of an initiator in a volatile solvent, allowing the solvent to evaporate, and then immersing the article in a solution of an acrylic monomer before subjecting the article to ultraviolet irradiation in air or an inert atmosphere.
- Acrylic acid is used as the acrylic monomer in each one of the Examples disclosed in the publication, although the use of equivalent amounts of methacrylic acid, acrylamide and other acrylic monomers is anticipated.
- the publication of Choi (2005) discloses a non-woven sheet of polyolefin fibres where opposed surfaces of the sheet are hydrophilic as a consequence of an acrylic graft polymerisation.
- the properties of the sheet are asymmetric, the ion exchange coefficient of the two surfaces being different.
- the method used to prepare these asymmetric acrylic graft polymerised non-woven polyolefin sheets comprises the steps of immersing the substrates in a solution of benzophenone (a photoinitiator), drying and then immersing the substrate in a solution of acrylic acid prior to subjecting to ultraviolet (UV) irradiation.
- UV ultraviolet
- the irradiation may be performed when the surfaces are in contact with either air or an inert atmosphere .
- Gao et al (2013) discloses a method of preparing a radiation cross-linked lithium-ion battery separator.
- a porous polyethylene membrane is immersed in a solution of benzophenone and triallyl cyanurate in dichloromethane .
- the immersed membrane is dried at room temperature before being immersed in a water bath at 30°C and irradiated on both sides using a high-pressure mercury lamp for three minutes .
- polyethylene membrane using an ultraviolet radiation energy source The grafted membranes are proposed for use in removing charged contaminants from liquids .
- the objective of the majority of these prior art methods is to improve the adhesion, biocompatibility, printability or wettability of the surface of a substrate using photoinitiated polymerisation. These methods are to be distinguished from the use of UV-initiated grafting with an exogenously prepared preformed polymer to modify the permeability to water of a hydrophobic microporous polyolefin substrate.
- the publication of Exley (2016) discloses an asymmetric composite membrane consisting of a film of cross-linked poly (ether ether ketone) adhered to a sheet of grafted microporous poly ( ethylene ) .
- the microporous poly ( ethylene ) is obtained by photoinitiated grafting with an ethenyl monomer to provide a hydrophilic sheet.
- the publication of Craft et al (2017) discloses improvements in the asymmetric composite membranes disclosed in the publication of Exley (2016) .
- the improved asymmetric composite membranes comprise of poly (vinyl alcohol) polymer crosslinked with a crosslinking agent (such as divinyl benzene) coated on a film of cross-linked poly (ether ether ketone) adhered to a sheet of the grafted microporous poly ( ethylene ) .
- the improvement is in the selectivity of the asymmetric composite membrane obtained.
- the invention provides a hydrophilicitized microporous sheet of polyolefin where the microporous polyolefin has been grafted with a preformed poly ( 4-ethenyl benzene sulfonic acid) .
- the polyolefin is selected from the group consisting of:
- the polyolefin is poly ( ethylene ) or poly (propylene ) .
- the polyolefin is poly ( ethylene ) .
- the preformed poly 4-ethenyl benzene sulfonic acid) is equivalent to that provided in the working solution prepared according to Example 1.
- the invention provides an asymmetric composite membrane comprising a film of partially crosslinked poly ( ethenol ) adhered to a hydrophilicitized microporous sheet of polyolefin where the polyolefin has been grafted with a preformed poly ( 4-ethenyl benzene sulfonic acid) before adherence of the film of partially crosslinked poly ( ethenol ) .
- the partially crosslinked poly ( ethenol ) is crosslinked to a degree in the range equivalent to that of the partially crosslinked poly ( ethenol ) provided in Vial 2 of Example 8 to that of the partially crosslinked poly ( ethenol ) provided in Vial 4 of Example 8. More preferably, the partially crosslinked poly ( ethenol ) is crosslinked to a degree substantially equivalent to that of the partially crosslinked poly ( ethenol ) provided in Vial 3 of Example 8.
- the polyolefin is selected from the group consisting of:
- polystyrene resin polystyrene resin
- polyolefin is poly ( ethylene ) or poly (propylene )
- polyolefin is poly ( ethylene ) .
- the invention provides an asymmetric composite membrane consisting essentially of a film of partially crosslinked poly ( ethenol ) adhered to a hydrophilicitized microporous sheet of poly ( ethylene ) where the polyolefin has been grafted with a preformed poly ( 4-ethenyl benzene sulfonic acid) before adherence of the film of partially crosslinked poly ( ethenol ) .
- the invention provides an asymmetric composite membrane consisting essentially of a film of partially crosslinked poly ( ethenol ) adhered to a hydrophilicitized microporous sheet of poly ( ethylene ) where the polyolefin has been grafted with a preformed poly ( 4-ethenyl benzene sulfonic acid) equivalent to that provided in the working solution prepared according to Example 1 before adherence of the film of partially crosslinked poly ( ethenol ) and the partially crosslinked poly ( ethenol ) is crosslinked to a degree
- the invention provides a method of preparing the hydrophilicitized microporous sheet of polyolefin of the first aspect of the invention comprising the steps of:
- the polyolefin is selected from the group consisting of:
- polystyrene resin polystyrene resin
- polyolefin is poly ( ethylene ) or poly (propylene )
- polyolefin is poly ( ethylene ) .
- the aqueous solvent is acetone-water.
- the curing the contacted microporous sheet is by irradiating with ultraviolet light at an intensity and at a temperature for a period of time sufficient for at least a portion of the poly ( 4-ethenylbenzenesulfonic acid) to be grafted onto the polyolefin.
- the irradiating is in the presence of a photoinitiator. More preferably, the irradiating is in the presence of a photoinitiator selected from the group consisting of: aceto-phenone, anthraquinone, benzoin, benzoin ether, benzoin ethyl ether, benzil, benzil ketal, benzophenone, benzoyl peroxide, n-butyl phenyl ketone, iso-butyl phenyl ketone,
- the irradiating is in the presence of the photoinitiator benzophenone.
- the ultraviolet light has a broad spectrum centred on 250 nm and bandwidth limits of approximately 250 nm and 400 nm.
- the washing is with water.
- the invention provides a method of preparing a hydrophilicitized microporous sheet of poly ( ethylene ) comprising the steps of:
- radical initiator to provide a first dispersion in a first solvent of a poly ( 4-ethenylbenzenesulfonic acid);
- the 4-ethenylbenzenesulfonic acid may be provided in the form of a salt, e.g. as its sodium salt (SSS) .
- a salt e.g. as its sodium salt (SSS) .
- the radical initiator is selected from the group consisting of: ammonium persulfate and sodium persulfate. More preferably, the radical initiator is sodium persulfate.
- the second solvent is 40 to 60% (v/v) acetone in water. Most preferably, the second solvent is 50% (v/v) acetone in water.
- the second dispersion may be prepared by adding acetone to the first dispersion .
- the invention provides a hydrophilicitized microporous sheet of polyolefin prepared according to the method of the third aspect of the invention.
- the invention provides a method of preparing the asymmetric composite membrane of the second aspect of the invention, comprising the steps of:
- the drying of the contacted sheet is by applying a positive thermal gradient across the thickness of the sheet from the contacted one side of the hydrophilicitized microporous sheet to the other side.
- crosslinking agent means a material that is incorporated into the crosslinking bridge of a cross-linked polymer network
- flux means the rate (volume per unit of time) of permeate transported per unit of membrane area
- graft polymer means a polymer in which the linear main chain has attached to it at various points side chains of a structure different from the main chain
- homopolymer means a polymer formed by the polymerization of a single monomer
- hydrophilic means having a tendency to mix with, dissolve in, or be wetted by water and “hydrophilicity"
- microporous means consisting of an essentially continuous matrix structure containing substantially uniform small pores or channels throughout the body of the substrate (such as may be manufactured using a cast (wet) process technology) and specifically excludes a discontinuous matrix of woven or non-woven fibres;
- partially crosslinked means that only a portion of the available sites for cross-linking are utilised and the cross-linking reaction has been limited by reagents, temperature or period of time;
- photoinitiator means a photolabile compound which upon irradiation forms a radical;
- poly ( ethanol ) and “polyvinyl alcohol” are used synonymously;
- post-treated polymer means a polymer that is modified, either partially or completely, after the basic polymer backbone has been formed;
- preformed means formed beforehand, i.e. prior to treatment;
- PSSS or "pSSS” denotes the product of the polymerization of SSS, i.e. poly ( 4-ethenylbenzenesulfonic acid);
- PVA denotes poly ( ethenol ) (or polyvinyl alcohol);
- SSLS denotes sodium styrene sulfonate, i.e. the sodium salt of 4-ethenylbenzenesulfonic acid;
- UVA means electromagnetic radiation having wavelengths between 320 and 400 nm;
- UVB means
- UVC electromagnetic radiation having wavelengths between 200 and 290 nm
- xPVA denotes PVA that is at least partially crosslinked.
- PSSS PSSS
- BP photoinitiator benzophenone
- no washing protocol (1) washed with water at a temperature of 45 to 50°C before drying (2), washed with acetone (3) and washed with water at a temperature of 45 to 50°C, dried and then washed with acetone (4) .
- poly ( ethenol ) (xPVA) prepared according the Example 8. From left to right:
- Figure 7 Comparison of the FTIR spectra (stretch mode region) recorded for samples (240818Si and 240818Sii) of an asymmetric composite membrane prepared according to Example 9 and the poly ( ethenol ) (PVA) and cross- linked poly ( ethenol ) (xPVA) used in their preparation.
- PVA poly ( ethenol )
- xPVA cross- linked poly
- Figure 8 Comparison of the FTIR spectra (finger print region) recorded for samples (240818Si and 240818Sii) of an asymmetric composite membrane prepared according to Example 9 and the poly ( ethenol ) (PVA) and cross- linked poly ( ethenol ) (xPVA) used in their preparation.
- PVA poly ( ethenol )
- xPVA cross- linked poly ( ethenol )
- FIG. 9 Scanning electronmicrographs of the surface of samples of asymmetric composite membrane prepared according to Example 9 before and after being subjected to repeated clean-in-place (CIP) protocols.
- the invention resides in part in the selection of a preformed polymer of 4- ethenylbenzenesulfonic acid as the hydrophilicitizing agent used in the preparation of hydrophilicitized polyolefin substrates.
- This part of the invention is most advantageously applied to the hydrophilicitization of preformed sheets of microporous poly ( ethylene ) .
- Use of poly (4- ethenylbenzenesulfonic acid) as the hydrophilicitizing agent has been found to provide greater and more consistent hydrophilicitization of the polyolefin substrate. This improvement is attributed at least in part to the reduced number of side reactions that may occur when compared with use of the monomer (cf. the method described in the publications of Exley (2016) and Craft et al (2017) ) . It is also anticipated that the use increases the likelihood of the preformed polymer grafting to the polyolefin substrate at multiple sites. A structurally distinct form of grafted polyolefin substrate may therefore be being obtained.
- hydrophilicitized sheet of microporous poly ( ethylene ) prepared by the method of the present invention when compared with that prepared by the method disclosed in the publications of Exley (2016) and Craft et al (2017) is demonstrated by a higher flux with water as the feed stream whilst retaining the desired durability including tolerance to chlorine and other cleaning agents.
- the hydrophilicitized sheets of microporous poly ( ethylene ) prepared by the method of the present invention also "wet out” at pressures lower than those previously required.
- the method of preparing the hydrophilicitized sheets of microporous poly ( ethylene ) is also less wasteful of reagents, including the
- the polymer of 4-ethenylbenzenesulfonic acid is a polymer of 4-ethenylbenzenesulfonic acid
- the invention also resides in part in the use of the hydrophilicitized sheet of microporous polyolefin to prepare an asymmetric composite membrane.
- microporous polyolefin facilitates the formation of the film of partially cross-linked poly ( ethenol ) (xPVA) on the surface and adherence to that surface.
- xPVA partially cross-linked poly
- persulfate is used as a cross-linking agent.
- the high levels of protein rejection demonstrated for the asymmetric composite membranes is attributed in part to the selection of this crosslinking agent.
- a porosity providing a size exclusion reduced to an estimated 30 kDa from an estimated 160 kDa is believed to be achieved (and is supported by the increased levels of total protein rejection of greater than 99.9%) .
- asymmetric composite membranes provided by the invention are therefore further distinguished from other membranes, e.g. those suggested in the publication of Linder et al (1988), where a superficial film of cross- linked PVA or PVA-copolymer is proposed to be coated on a hydrophobic, i.e. water repelling, sheet of microporous polyolefin.
- microporous sheets used in the preparation of samples were prepared from virgin poly ( ethylene ) , i.e. poly ( ethylene ) of high purity.
- Spectra of the samples were recorded using a Thermo Electron Nicolet 8700 FTIR spectrometer equipped with a single bounce ATR and diamond crystal. An average of 32 scans with a 4 crrr 1 resolution was taken for all samples.
- Permeability was determined using a filter assembly (Sterlitech Corp.) by measuring the flux with deionized water as the feed stream at various pressures. Flux J v was then graphed against effective pressure difference across the membrane, p eff , and the slope of the permeability L p .
- the samples were mounted in the filter assembly. Deionized water was fed into the rig at 2.5 L min -1 and 4 to 8 °C. The time to collect a
- V is the permeate volume (L)
- t is the time (h) for the collection of V
- A is area of the sample (m 2 ) which was determined to be 0.014 m 2 .
- Rejection was measured using a 2 g/L solution in water of sodium chloride with a feed pressure of 16 bar. The conductivities from the feed and permeate were compared. 100
- Rejection for whole milk samples was measured by pouring 20 mL of sample from the feed in a petri dish and measuring the dry weight after 2 hours in a 100 °C oven.
- m P TS is total milk solids in the permeate and h 3 ⁇ 4 T5 is the mass of milk total solids in the feed.
- Total protein and total whey protein concentrations in permeate were calculated on the basis of HPLC analysis with UV absorbance monitoring.
- the membrane was subjected to a first wash by circulating a 2% (w/v) sodium hydroxide solution ("caustic wash") through the filter assembly for a period of five minutes before draining and flushing the system by
- the membrane was subjected to a second wash by circulating a 2% (w/w) nitric acid solution ("acid wash") through the filter assembly system for a period of ten minutes before draining and flushing the system of circulating water at an initial temperature of 65°C for a period of ten minutes.
- the membrane was subjected to a third wash (a "caustic wash") before flushing the system by
- a quantity of 50 g of the monomer 4-ethenylbenzenesulfonic acid as its sodium salt (SSS) was dissolved in a volume of 100 mL of distilled water to provide a solution.
- a quantity of 0.5 g of the initiator sodium persulfate (SPS) was then dissolved in the solution and the initiator-monomer mixture heated with stirring at a temperature of 80 to 90°C for a time of about 20 minutes.
- a viscous solution was obtained having a total volume of about 125 mL .
- the viscous solution was diluted with the same volume of distilled water to provide 250 mL of a working solution of poly (4- ethenylbenzenesulfonic acid) .
- the polymer could be precipitated from this working solution by the addition of an excess volume of acetone, followed by collection of the precipitate by filtration through a Buchner funnel and then washing with acetone to provide a light white solid that could be readily ground to a powder using a pestle and mortar.
- a quantity of 5 g of the monomer 4-ethenylbenzenesulfonic acid as its sodium salt (SSS) was dissolved in a volume of 20 mL of dimethylsulfoxide (DMSO) to provide a solution.
- SSS monomer 4-ethenylbenzenesulfonic acid as its sodium salt
- a quantity of 0.05 g of the initiator ammonium persulfate (APS) was then dissolved in the solution and the initiator-monomer mixture heated with stirring at a temperature of 80 to 90°C for a time of about 20 minutes.
- the poly ( 4-ethenylbenzenesulfonic acid) was precipitated from the cooled solution by addition of an excess volume of acetone, collected by
- FTIR Fourier transform infrared
- a volume of 6 mL of the working solution obtained according to Example 1 was mixed with a volume of 5 mL of distilled water in a vial to provide a volume of initial solution containing 1.2 g of poly (4- ethenylbenzenesulfonic acid) (pSSS) .
- pSSS poly (4- ethenylbenzenesulfonic acid)
- a volume of 10 mL acetone was added to the volume of initial solution and allowed to become transparent before adding and dissolving in the solution a quantity of 0.2 g of the
- Example 3 The method of preparation described in Example 3 was repeated with the volume of initial solution containing 1.7 g of poly ( 4- ethenylbenzenesulfonic acid) . This quantity of the polymer was close to the maximum that could be dissolved in the solvent system used.
- a one step method of preparation including the monomer 4- ethenylbenzenesulfonic acid was evaluated.
- a volume of 3 mL of the working solution obtained according to Example 1 was mixed with a volume of 8 mL of distilled water and a quantity of 0.6 g of the monomer 4-ethenylbenzenesulfonic acid in a vial to provide a volume of initial solution containing 0.6 g of poly ( 4-ethenylbenzenesulfonic acid) .
- a volume of 10 mL acetone was added to the volume of this initial solution and allowed to become transparent before adding a quantity of 0.4 g of the photoinitiator benzophenone to provide a hydrophilicitizing mixture .
- a sheet of microporous poly ( ethylene ) (TARGRAYTM wet process polyethylene separators, item no. SW320H (Targray, Kirkland QC, Canada) dimensioned (13.5 cm x 18.5 cm) to fit the filter assembly (Sterlitech Corp.) was contacted with the hydrophilicitizing mixture and irradiated with UV light (broad spectrum centred on 350 nm) for a period of time of 2 minutes before being washed with cold tap water and placed in a water bath maintained at a temperature of 45 to 50°C for about 5 minutes and then air dried .
- UV light broad spectrum centred on 350 nm
- a volume of 10 mL of distilled water followed by a volume of 10 mL of acetone was added to a foil wrapped vial containing a quantity of 2.4 g of the monomer and a quantity of 0.4 g of the photoinitiator benzophenone and the mixture shaken until all solids had dissolved.
- SW320H (Targray, Kirkland QC, Canada) dimensioned (13.5 cm x 18.5 cm) to fit the filter assembly of a test rig (Sterlitech Corp.) was contacted with the mixture and irradiated with ultraviolet (UV) light (broad spectrum centred on 350 nm) before washing with cold tap water and placing in a water bath maintained at a temperature of 45 to 50°C for a time of 5 minutes before being air dried.
- UV ultraviolet
- a volume of 6 mL of the working solution obtained according to Example 1 was mixed with a volume of 5 mL of distilled water in a vial to provide a volume of initial solution containing 1.2 g of poly ( 4-ethenylbenzenesulfonic acid) .
- a volume of 10 mL acetone was added to the volume of initial solution and allowed to become transparent before adding and dissolving in the solution a quantity of 0.2 of the
- photoinitiator benzophenone to provide a hydrophilicitizing mixture.
- the surface of the air dried sheet obtained according to the first step was contacted with the hydrophilicitizing mixture and irradiated with UV light (broad spectrum centered on 350 nm) for a period of time of 2 minutes before washing with cold tap water and placing in a water bath maintained at a temperature of 45 to 50°C for a period of time of about 5 minutes and then air dried.
- a series of preliminary experiments were performed to evaluate methods of preparing a film of cross-linked poly ( ethenol ) (xPVA) on a surface.
- a solution of the radical initiator sodium persulfate (SPS) was prepared by adding a quantity of 0.2 g of SPS to a volume consisting of 10 mL deionised water and 10 mL acetone. The solution of radical initiator was applied onto the surface of each of three glass plates (Plate 1, Plate 2 and Plate 3) . Plate 2 and Plate 3 were transferred to an oven and dried at a temperature of 60°C until all solvent had evaporated to leave a thin layer of the initiator deposited on the surface.
- Solutions of poly ( ethenol ) (PVA) were prepared at a concentration of 1% (w/v) in either dimethyl sulfoxide (DMSO) or deionised water.
- DMSO dimethyl sulfoxide
- the solution of poly ( ethenol ) (PVA) in DMSO was sprayed onto the wet surface of Plate 1 and the plate then transferred to an oven and dried at a temperature of 60°C.
- the solution of poly ( ethenol ) (PVA) in DMSO was also sprayed onto the dry surface of Plate 2 and the plate then transferred to an oven and dried at a temperature of 60°C.
- the solution of poly ( ethenol ) in deionised water was sprayed onto the dry surface of Plate 3 and the plate then transferred to an oven and dried at a temperature of 60°C.
- the desired film of cross-linked poly ( ethenol ) was not formed on Plate 1.
- the film formed on Plate 2 was too frangible to be useful as a rejection layer of an asymmetric composite membrane.
- SPS sulfur persulfate
- xPVA partially cross-linked poly ( ethenol )
- the solution of the radical initiator was applied to one surface of a hydrophilicitized sheet of microporous poly ( ethylene ) prepared according to Example 3. The sheet was then placed on a glass plate and transferred to an oven and dried at a temperature of 60°C. The solution of partially cross- linked poly ( ethenol ) was applied to the same surface of the dried sheet and the sheet then returned to the oven and dried at 60°C. The dried membrane was then washed with cool water and air dried before evaluation for flux, total solids and salts rejection with different feed streams (water and milk) . Evaluation of samples of asymmetric composite membrane
- PCT/GB92/ 01245 (publ. no. WO 93/01622).
Landscapes
- Chemical & Material Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Inorganic Chemistry (AREA)
- Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Health & Medical Sciences (AREA)
- Transplantation (AREA)
- Separation Using Semi-Permeable Membranes (AREA)
- Manufacture Of Porous Articles, And Recovery And Treatment Of Waste Products (AREA)
- Graft Or Block Polymers (AREA)
- Laminated Bodies (AREA)
Priority Applications (11)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| SG11202009651QA SG11202009651QA (en) | 2018-03-30 | 2019-04-01 | Asymmetric composite membranes and modified substrates used in their preparation |
| NZ767051A NZ767051B2 (en) | 2018-03-30 | 2019-04-01 | Asymmetric composite membranes and modified substrates used in their preparation |
| GB2017215.1A GB2586107B (en) | 2018-03-30 | 2019-04-01 | Asymmetric composite membranes and modified substrates used in their preparation |
| CN201980031056.4A CN112739450A (zh) | 2018-03-30 | 2019-04-01 | 不对称复合膜及其制备中使用的改性基材 |
| JP2020552852A JP7292742B2 (ja) | 2018-03-30 | 2019-04-01 | 非対称複合膜およびその調製に使用される修飾された基質 |
| EP19777936.6A EP3774004A4 (en) | 2018-03-30 | 2019-04-01 | COMPOSITE ASYMMETRIC MEMBRANE AND MODIFIED SUBSTRATES USED IN THEIR MANUFACTURE |
| AU2019246749A AU2019246749B2 (en) | 2018-03-30 | 2019-04-01 | Asymmetric composite membranes and modified substrates used in their preparation |
| AU2020233616A AU2020233616A1 (en) | 2018-03-30 | 2020-09-14 | Asymmetric composite membranes and modified substrates used in their preparation |
| IL277668A IL277668B (en) | 2018-03-30 | 2020-09-29 | Symmetrical composite membranes and modified substrates used in their preparation |
| US17/060,849 US12083780B2 (en) | 2018-03-30 | 2020-10-01 | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation |
| US18/828,567 US20250018347A1 (en) | 2018-03-30 | 2024-09-09 | Durable water permeable filtration membranes |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| AU2018901072 | 2018-03-30 | ||
| AU2018901072A AU2018901072A0 (en) | 2018-03-30 | Modified polymers |
Related Child Applications (2)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/IB2020/053116 Continuation-In-Part WO2020202044A1 (en) | 2018-03-30 | 2020-04-01 | Composite membranes |
| US17/060,849 Continuation-In-Part US12083780B2 (en) | 2018-03-30 | 2020-10-01 | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2019186518A1 true WO2019186518A1 (en) | 2019-10-03 |
Family
ID=68058626
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/IB2019/052649 Ceased WO2019186518A1 (en) | 2018-03-30 | 2019-04-01 | Asymmetric composite membranes and modified substrates used in their preparation |
Country Status (8)
| Country | Link |
|---|---|
| EP (1) | EP3774004A4 (cg-RX-API-DMAC7.html) |
| JP (1) | JP7292742B2 (cg-RX-API-DMAC7.html) |
| CN (1) | CN112739450A (cg-RX-API-DMAC7.html) |
| AU (2) | AU2019246749B2 (cg-RX-API-DMAC7.html) |
| GB (1) | GB2586107B (cg-RX-API-DMAC7.html) |
| IL (1) | IL277668B (cg-RX-API-DMAC7.html) |
| SG (1) | SG11202009651QA (cg-RX-API-DMAC7.html) |
| WO (1) | WO2019186518A1 (cg-RX-API-DMAC7.html) |
Cited By (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN111495217A (zh) * | 2020-04-14 | 2020-08-07 | 北京上远科技有限公司 | 一种表面改性耐污染复合纳滤膜的制备方法 |
| WO2020202044A1 (en) * | 2019-04-01 | 2020-10-08 | Hydroxsys Holdings Limited | Composite membranes |
| US20210016554A1 (en) * | 2018-03-30 | 2021-01-21 | Hydroxsys Holdings Limited | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation |
| CN118874240A (zh) * | 2024-09-18 | 2024-11-01 | 山东大学 | 一种致密聚酰胺Janus膜蒸馏膜及其制备方法和应用 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2008043507A1 (en) * | 2006-10-11 | 2008-04-17 | Lydall Solutech B.V. | Humidifier membrane |
| US20130116589A1 (en) * | 2009-03-03 | 2013-05-09 | Oridion Medical (1987) Ltd. | Drying substances, preparation and use thereof |
| WO2016081729A1 (en) * | 2014-11-20 | 2016-05-26 | Entegris, Inc. | Grafted ultra high molecular weight polyethylene microporous membranes |
| WO2016103239A1 (en) * | 2014-12-24 | 2016-06-30 | Mark Exley | Asymmetric composite membranes and modified substrates used in their preparation |
| WO2017056074A1 (en) * | 2015-10-01 | 2017-04-06 | Craft Lenka Benacek | Asymmetric composite membrane and a method of preparation thereof |
Family Cites Families (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP3741871B2 (ja) | 1998-08-12 | 2006-02-01 | 日本原子力研究所 | 放射線グラフト重合方法 |
| AU2001259213A1 (en) * | 2000-04-28 | 2001-11-12 | Puradyn Filter Technologies Incorporated | Improved filtration efficiency |
| JP4229421B2 (ja) * | 2000-11-02 | 2009-02-25 | 等 金澤 | 高分子材料の改質方法およびその用途 |
| JP4384444B2 (ja) | 2003-05-29 | 2009-12-16 | 株式会社荏原製作所 | 電気式脱塩装置及び電気透析装置 |
| JP2008514735A (ja) | 2004-09-27 | 2008-05-08 | 株式会社荏原製作所 | グラフト材料及びその製造方法 |
| DE102013200120A1 (de) * | 2013-01-08 | 2014-07-10 | PolyAn Gesellschaft zur Herstellung von Polymeren für spezielle Anwendungen und Analytik mbH | Verfahren zur Herstellung eines Kunststoffartikels mit hydrophober Pfropfbeschichtungsowie Kunststoffartikel |
| CN103816816B (zh) * | 2014-02-28 | 2016-02-03 | 中国科学院长春应用化学研究所 | 一种聚合物膜材料及其制备方法 |
| CN105498554A (zh) * | 2016-02-01 | 2016-04-20 | 常州市君成机械有限公司 | 一种辐照紫外接枝改性高截留率纳滤膜的制备方法 |
| JP2019085502A (ja) * | 2017-11-08 | 2019-06-06 | 王子ホールディングス株式会社 | 成形体用基材、および成形体用基材の製造方法 |
-
2019
- 2019-04-01 GB GB2017215.1A patent/GB2586107B/en active Active
- 2019-04-01 EP EP19777936.6A patent/EP3774004A4/en not_active Withdrawn
- 2019-04-01 CN CN201980031056.4A patent/CN112739450A/zh active Pending
- 2019-04-01 JP JP2020552852A patent/JP7292742B2/ja active Active
- 2019-04-01 WO PCT/IB2019/052649 patent/WO2019186518A1/en not_active Ceased
- 2019-04-01 SG SG11202009651QA patent/SG11202009651QA/en unknown
- 2019-04-01 AU AU2019246749A patent/AU2019246749B2/en not_active Ceased
-
2020
- 2020-09-14 AU AU2020233616A patent/AU2020233616A1/en not_active Abandoned
- 2020-09-29 IL IL277668A patent/IL277668B/en unknown
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2008043507A1 (en) * | 2006-10-11 | 2008-04-17 | Lydall Solutech B.V. | Humidifier membrane |
| US20130116589A1 (en) * | 2009-03-03 | 2013-05-09 | Oridion Medical (1987) Ltd. | Drying substances, preparation and use thereof |
| WO2016081729A1 (en) * | 2014-11-20 | 2016-05-26 | Entegris, Inc. | Grafted ultra high molecular weight polyethylene microporous membranes |
| WO2016103239A1 (en) * | 2014-12-24 | 2016-06-30 | Mark Exley | Asymmetric composite membranes and modified substrates used in their preparation |
| WO2017056074A1 (en) * | 2015-10-01 | 2017-04-06 | Craft Lenka Benacek | Asymmetric composite membrane and a method of preparation thereof |
Non-Patent Citations (1)
| Title |
|---|
| BOLTO, B. ET AL.: "Crosslinked poly(vinyl alcohol) membranes", PROGRESS IN POLYMER SCIENCE, vol. 34, 2009, pages 969 - 981, XP026546549, doi:10.1016/j.progpolymsci.2009.05.003 * |
Cited By (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US20210016554A1 (en) * | 2018-03-30 | 2021-01-21 | Hydroxsys Holdings Limited | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation |
| US12083780B2 (en) * | 2018-03-30 | 2024-09-10 | Hydroxsys Holdings Limited | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation |
| WO2020202044A1 (en) * | 2019-04-01 | 2020-10-08 | Hydroxsys Holdings Limited | Composite membranes |
| CN111495217A (zh) * | 2020-04-14 | 2020-08-07 | 北京上远科技有限公司 | 一种表面改性耐污染复合纳滤膜的制备方法 |
| CN111495217B (zh) * | 2020-04-14 | 2022-07-08 | 北京上远科技有限公司 | 一种表面改性耐污染复合纳滤膜的制备方法 |
| CN118874240A (zh) * | 2024-09-18 | 2024-11-01 | 山东大学 | 一种致密聚酰胺Janus膜蒸馏膜及其制备方法和应用 |
Also Published As
| Publication number | Publication date |
|---|---|
| EP3774004A4 (en) | 2022-05-04 |
| SG11202009651QA (en) | 2020-10-29 |
| GB2586107B (en) | 2021-12-22 |
| AU2020233616A1 (en) | 2020-10-08 |
| NZ767051A (en) | 2021-10-29 |
| AU2019246749B2 (en) | 2020-10-29 |
| GB2586107A (en) | 2021-02-03 |
| EP3774004A1 (en) | 2021-02-17 |
| AU2019246749A1 (en) | 2020-07-23 |
| IL277668B (en) | 2022-03-01 |
| JP2021519686A (ja) | 2021-08-12 |
| JP7292742B2 (ja) | 2023-06-19 |
| CN112739450A (zh) | 2021-04-30 |
| IL277668A (en) | 2020-11-30 |
| GB202017215D0 (en) | 2020-12-16 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| AU2017254972B2 (en) | Asymmetric composite membranes and modified substrates used in their preparation | |
| AU2020233616A1 (en) | Asymmetric composite membranes and modified substrates used in their preparation | |
| WO2020202044A1 (en) | Composite membranes | |
| JP5120543B2 (ja) | 陽イオン交換膜およびその製造方法 | |
| Liu et al. | Hydrophilic modification of P (VDF-co-CTFE) porous membranes | |
| US11389771B2 (en) | Asymmetric composite membrane and a method of preparation thereof | |
| US11291215B2 (en) | Durable asymmetric composite membranes and modified substrates used in their preparation | |
| US12083780B2 (en) | Asymmetric composite membranes and hydrophilicitized microporous sheets of polyolefin used in their preparation | |
| US20220193620A1 (en) | Asymmetric composite membranes and modified substrates used in their preparation | |
| US20220161204A1 (en) | Durable membranes, their preparation and use | |
| NZ767051B2 (en) | Asymmetric composite membranes and modified substrates used in their preparation | |
| CN115151336B (zh) | 耐用膜及其制备和用途 | |
| JP3626650B2 (ja) | イオン性膜の製造方法 | |
| US20250018347A1 (en) | Durable water permeable filtration membranes | |
| NZ733706B (en) | Asymmetric composite membranes and modified substrates used in their preparation |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 19777936 Country of ref document: EP Kind code of ref document: A1 |
|
| DPE1 | Request for preliminary examination filed after expiration of 19th month from priority date (pct application filed from 20040101) | ||
| ENP | Entry into the national phase |
Ref document number: 2019246749 Country of ref document: AU Date of ref document: 20190401 Kind code of ref document: A |
|
| ENP | Entry into the national phase |
Ref document number: 2020552852 Country of ref document: JP Kind code of ref document: A |
|
| ENP | Entry into the national phase |
Ref document number: 202017215 Country of ref document: GB Kind code of ref document: A Free format text: PCT FILING DATE = 20190401 |
|
| ENP | Entry into the national phase |
Ref document number: 2019777936 Country of ref document: EP Effective date: 20201030 |
|
| WWW | Wipo information: withdrawn in national office |
Ref document number: 2019777936 Country of ref document: EP |