WO2014100487A2 - Methods to bond silica parts - Google Patents

Methods to bond silica parts Download PDF

Info

Publication number
WO2014100487A2
WO2014100487A2 PCT/US2013/076708 US2013076708W WO2014100487A2 WO 2014100487 A2 WO2014100487 A2 WO 2014100487A2 US 2013076708 W US2013076708 W US 2013076708W WO 2014100487 A2 WO2014100487 A2 WO 2014100487A2
Authority
WO
WIPO (PCT)
Prior art keywords
crucible
weir
melt
silica
base
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2013/076708
Other languages
English (en)
French (fr)
Other versions
WO2014100487A3 (en
Inventor
Richard J. Phillips
Shailendra B. Rathod
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SunEdison Inc
Original Assignee
SunEdison Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SunEdison Inc filed Critical SunEdison Inc
Priority to CN201380066117.3A priority Critical patent/CN104870394A/zh
Priority to JP2015549738A priority patent/JP2016505503A/ja
Publication of WO2014100487A2 publication Critical patent/WO2014100487A2/en
Publication of WO2014100487A3 publication Critical patent/WO2014100487A3/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B15/00—Single-crystal growth by pulling from a melt, e.g. Czochralski method
    • C30B15/10—Crucibles or containers for supporting the melt
    • C30B15/12—Double crucible methods
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03B—MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES
    • C03B23/00—Re-forming shaped glass
    • C03B23/20—Uniting glass pieces by fusing without substantial reshaping
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C27/00—Joining pieces of glass to pieces of other inorganic material; Joining glass to glass other than by fusing
    • C03C27/06—Joining glass to glass by processes other than fusing
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B15/00—Single-crystal growth by pulling from a melt, e.g. Czochralski method
    • C30B15/002—Continuous growth
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B15/00—Single-crystal growth by pulling from a melt, e.g. Czochralski method
    • C30B15/20—Controlling or regulating
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B29/00—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape
    • C30B29/02—Elements
    • C30B29/06—Silicon
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C2217/00—Coatings on glass
    • C03C2217/20—Materials for coating a single layer on glass
    • C03C2217/21—Oxides
    • C03C2217/213—SiO2
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T117/00—Single-crystal, oriented-crystal, and epitaxy growth processes; non-coating apparatus therefor
    • Y10T117/10—Apparatus
    • Y10T117/1024—Apparatus for crystallization from liquid or supercritical state
    • Y10T117/1032—Seed pulling
    • Y10T117/1052—Seed pulling including a sectioned crucible [e.g., double crucible, baffle]

Definitions

  • This disclosure generally relates to methods for bonding silica parts, and to silica crucibles used for growing single-crystal ingots.
  • polycrystalline silicon is first melted within a crucible, such as a quartz crucible, of a crystal pulling device to form a silicon melt.
  • a seed crystal is lowered into the melt and slowly raised out of the melt to produce a silicon ingot.
  • the temperature and the stability of the surface of the melt immediately adjacent to the ingot must be maintained substantially constant. There is a need for a more effective system and method to limit temperature fluctuation and surface disruptions in the melt immediately adjacent to the ingot .
  • a first aspect is a method of bonding a first silica part to a second silica part. The method
  • first and second silica parts includes providing the first and second silica parts; coating contacting surfaces of the first silica part and second silica part with a solution having at least one of silica and silica precursors; placing the coated surfaces of the first silica part adjacent to the coated surfaces of the second silica part to form an assembly; and heating the assembly.
  • the crucible for use in directional solidification of multicrystalline ingots.
  • the crucible has a base, a sidewall extending around the base to form a vessel for the containment of material therein, and a weir attached to the base at a location inward from the sidewall to define an inner cavity and an outer cavity.
  • the weir has at least one passage therethrough to allow material in the outer cavity to be moved to the inner cavity.
  • Still another aspect is a system for growing a single crystal ingot.
  • the system includes a crucible, a heater, and a feed tube.
  • the crucible has a base, a sidewall extending about the base to form a vessel for the containment of material therein, and a weir affixed to the base at a location inward from the sidewall to define an inner cavity and an outer cavity.
  • the weir has at least one passage therethrough to allow material in the outer cavity to be moved to the inner cavity.
  • the heater is located adjacent to the crucible for supplying heat to the crucible to
  • the feed tube is connected with the crucible for supplying a feedstock material to the crucible .
  • Yet another aspect is a method for growing a single crystal ingot from a crucible having a base, a sidewall and a weir affixed to the base at a location inward from the sidewall to define an inner cavity and an outer cavity, the weir having at least one passage
  • the method includes placing a feedstock material into the crucible; melting the feedstock material to form a melt that passes through the passage from the outer cavity to the inner cavity; lowering a seed crystal into the melt; and pulling the seed crystal from the melt to pull an ingot from the seed crystal.
  • Figure 1 is a partial cross sectional view of a crucible in accordance with one embodiment
  • Figure 2 is a schematic side view of a crystal growing system in accordance with another embodiment.
  • Figure 3 is a partial cross sectional view of a crucible in accordance with another embodiment.
  • a crucible for use in directional solidification of multicrystalline ingots is shown and indicated generally at 100.
  • the crucible 100 has a base 110, a sidewall 120, and a weir 130.
  • the sidewall 120 extends upward around a perimeter 112 of the base to form a concave hollow 102 in crucible 100 for the containment of material therein.
  • the weir 130 is affixed to the base 110 by a bonding agent 140.
  • the affixed weir 130 extends upward from a top surface 114 of the base 110 at a location radially inward from the sidewall 120.
  • the weir 130 separates the concave hollow 102 into an inner cavity 104 and an outer cavity 106.
  • a passage 132 extends through the weir 130 to connect the inner cavity 104 and the outer cavity 106.
  • Weir 130 may be a cylindrical body or any other suitable shape.
  • contacting surfaces of the parts are made to have a similar contour and to mate together.
  • the contacting surfaces of each part are coated with solution containing silica or silica precursors (e.g., "slip").
  • the solution is prepared to develop a dispersed colloidal suspension and is typically brushed onto both sides of the contacting surfaces.
  • the contacting surfaces are then pressed together and allowed to dry.
  • the solution is typically an aqueous based system, so the solution is allowed to air dry.
  • the joint After air drying, the joint is placed into a heating source capable of heating the parts to a specified temperature range, under controlled conditions to minimize devitrification, to bond the two surfaces together.
  • the controlled conditions are such that the crystalline
  • the controlled conditions include heating the coated parts in an inert atmosphere, such as argon, - to a temperature in the range of about 1150° C to about 1550° C for between about 4 hours to almost 16 hours.
  • the time is based on obtaining adequate viscous flow at the joint to effect bonding. The actual time will depend on the continuity of the joint after heat treatment to minimize or eliminate void space between the joint.
  • the solution may include slip casting agents, such as Cab-0-Sil, Thermosil, or other suitable slip cast agents.
  • slip casting agents such as Cab-0-Sil, Thermosil, or other suitable slip cast agents.
  • the solution may include a silica precursor, such as tetroalkoxysilane or other suitable silica precursor.
  • a crystal growing system is shown in Figure 2 and indicated generally at 200.
  • the crystal growing system 200 is used to produce a large crystal or ingot by the Czochralski method.
  • the crystal growing system 200 includes the crucible 100 that contains a silicon melt 212 from which an ingot 214 is being pulled from the melt by a puller or puller system 234.
  • a seed crystal 232 is lowered by a puller 234 into a melt 212 and then slowly raised from the silicon melt.
  • silicon atoms from the melt align themselves with and attach to the seed crystal to form an ingot 214.
  • Feedstock material 216 may be placed into the outer cavity 106 of crucible 100, at a location radially outward from the weir, from feeder 218 through feed tube 220.
  • the feedstock material 216 is at a much lower temperature than the surrounding melt 212 and absorbs heat from the melt as the feedstock material's temperature rises, and as the feedstock material itself melts. As feedstock material 216 absorbs energy from melt 212, the temperature of the surrounding melt falls immediately. During these fluctuations of the melt temperature, the ability of the silicon atoms to properly align themselves is hindered.
  • feedstock material 216 added is controlled by feeder 218, which is responsive to
  • Controller 222 is a computing device for controlling the feed rate of the
  • the amount of cooling of the melt 212 is precisely determined and
  • Controller 222 either adds or does not add feedstock to adjust the temperature of the melt. As feedstock material 216 is added to melt 212, the surface of the melt may be disturbed. This disturbance also affects the ability of the melt silicon atoms to properly align with the silicon atoms of the seed crystal.
  • Heat is provided to crucible 100 by heaters 224, 226, and 228 located at various positions about the crucible. Heat from heaters 224, 226, and 228 melt or
  • Heater 224 is generally cylindrical in shape and provides heat to the sides of the crucible 100, and heaters 226 and 228 provide heat to the bottom of the
  • heaters 226 and 228 are generally annular in shape.
  • Heaters 224, 226, and 228 are resistive heaters coupled to controller 222, which controllably applies electric current to the heaters to alter their temperature.
  • a sensor 230 such as a pyrometer or like temperature sensor, provides a continuous measurement of the temperature of melt 212 at the crystal/melt interface of the growing single crystal ingot 214. Sensor 230 also may be directed to measure the temperature of the growing ingot. Sensor 230 is
  • controller 222 communicatively coupled with controller 222.
  • temperature sensors may be added to measure and provide temperature feedback to the controller with respect to points that are critical to the growing ingot. While a single communication lead is shown for clarity, one or more
  • temperature sensor (s) may be linked to the controller by multiple leads or a wireless connection, such as by an IR data link or other suitable connections.
  • the amount of current supplied to each of the heaters 224, 226, and 228 by controller 222 may be separately and independently chosen to optimize the thermal characteristics of melt 212.
  • one or more heaters may be disposed around the crucible to provide heat.
  • seed crystal 232 is attached to a portion of puller 234 located over melt 212.
  • the puller 234 provides movement of seed crystal 232 in a direction perpendicular to the surface of melt 212 allowing the seed crystal to be lowered down toward or into the melt, and raised up or out of the melt.
  • the melt 212 in an area adjacent to seed crystal 232/ingot 214 must be maintained at a substantially constant
  • the weir 130 limits the surface disturbances and temperature fluctuations in the area immediately adjacent to seed crystal 232/ingot 214. Residual solid silicon pieces are also inhibited from passing through the passage to the inner cavity.
  • more than one weir may be used within the crucible, which will increase the residence time of dissolvable or meltable particles in the outer cavities. Similar bonding methods may be used on each weir to obtain a similar benefit of
  • the movement of the melt 212 is limited to the location of the passage 132. Placing passage 132 along a lower section of the weir 130 confines the movement of melt 212 to movement along the base 110 of the crucible 100. Thus, any movement of melt 212 into the inner melt portion is distal from or opposite the top of the melt (where the ingot 214 is being pulled) . This confinement of the melt movement limits surface disruptions and temperature fluctuations along the top of the inner melt portion of the melt 212.
  • the passage 132 permits controlled movement of melt 212 between the outer cavity 106 and the inner cavity 104. Limiting the melt movement between the cavities 104, 106 allows the silicon material in the outer cavity 106 to heat to an approximately equivalent temperature of the melt in the inner cavity 104 as the silicon material passes through the passage 132.
  • silicon is melted in the outer cavity, while solid silicon is fed continuously into the outer cavity 106.
  • the melt 212 passes from the outer cavity 106 to the inner cavity 104 through the passage 132.
  • the ingot 214 is then grown from the melt 212 within the inner cavity 104.
  • the passage 132 may be disposed on the weir 130 at a location that is diametrically opposed to the feed tube 220 to increase the distance that feedstock material 216 must traverse before entering the inner cavity 104.
  • the weir and the feedstock material are placed in the crucible.
  • Heaters are placed adjacent to the crucible to provide heat for liquefying or melting the feedstock material forming a melt.
  • the seed crystal is lowered into and then slowly raised out of the melt to grow the ingot from the seed crystal .
  • feedstock material may be placed in both/either the inner cavity 104 and/or the outer cavity 106.
  • the feedstock material may be placed in an area outside of the weir 130 for a continuous process of feeding and crystal growth.
  • the melt 212 is allowed to move from the outer cavity 106 into the inner cavity 104.
  • the movement of the melt between the cavities 104, 106 is limited to passages through the outer leg and inner leg of the weir 130.
  • the weir 130 does not include passages therethrough.
  • the weir 130 is bonded to the crucible at discrete locations along the length of the weir, defining unbounded portions.
  • the unbounded portions form gaps, under the legs of the weir, between the weir and crucible. Movement of the melt from the outer cavity into the inner cavity is limited to movement through the gaps formed by the unbounded portions.
  • the melt entering the inner cavity 104 is substantially equivalent in temperature to the melt already in the inner cavity. Raising the temperature of the melt before reaching the inner cavity 104 reduces the temperature gradients within the inner cavity.
  • the controller acts to maintain a substantially constant temperature within the inner cavity 104.
  • the weir 130 substantially prevents disturbances in the outer cavity 106 from disrupting the surface of the melt in the inner cavity 104 by substantially containing the energy waves produced by the disturbances.
  • the disturbances are also limited by the location of the passage.
  • the passage is along the bottom of the crucible, which allows movement of the melt into the inner cavity 104 without disrupting the surface stability of the inner cavity.
  • the controller 222 is also capable of simultaneously supplying feedstock material while the seed crystal is raised from the melt and growing the ingot .
  • FIG. 3 another embodiment of a crucible for use in directional solidification of multicrystalline ingots is shown and indicated generally at 300.
  • the crucible 300 has a base 310, a sidewall 320, a first weir 330, and a second weir 350.
  • the first weir 330 is affixed to the base 310 by a bonding agent 340.
  • the second weir 350 is also affixed to the base 310 by a bonding agent 360.
  • both the first weir 330 and second weir 350 are affixed to the base 310 with bonding agents 340 and 360, respectively.
  • bonding agent 340 may be the same as bonding agent 360.
  • bonding agents 340 and 360 have different compositions.
  • Embodiments as described above enable increased yield and a better quality ingot, while decreasing the costs of the process.
  • An example system with Cab-O-Sil was determined to perform more than four times better than a control or no slip system. This determination was made by a line/intercept method of intersection of voids at the interface .

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Organic Chemistry (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Metallurgy (AREA)
  • Ceramic Engineering (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Geochemistry & Mineralogy (AREA)
  • Crystals, And After-Treatments Of Crystals (AREA)
  • Joining Of Glass To Other Materials (AREA)
  • Silicon Compounds (AREA)
PCT/US2013/076708 2012-12-21 2013-12-19 Methods to bond silica parts Ceased WO2014100487A2 (en)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN201380066117.3A CN104870394A (zh) 2012-12-21 2013-12-19 结合二氧化硅部件的方法、用于生长单晶锭的坩埚、系统及其方法
JP2015549738A JP2016505503A (ja) 2012-12-21 2013-12-19 シリカパーツを接合するための方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US201261740943P 2012-12-21 2012-12-21
US61/740,943 2012-12-21

Publications (2)

Publication Number Publication Date
WO2014100487A2 true WO2014100487A2 (en) 2014-06-26
WO2014100487A3 WO2014100487A3 (en) 2015-03-05

Family

ID=49920686

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2013/076708 Ceased WO2014100487A2 (en) 2012-12-21 2013-12-19 Methods to bond silica parts

Country Status (4)

Country Link
US (1) US20140174338A1 (enExample)
JP (1) JP2016505503A (enExample)
CN (1) CN104870394A (enExample)
WO (1) WO2014100487A2 (enExample)

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20250051957A1 (en) * 2023-08-11 2025-02-13 Globalwafers Co., Ltd. Crucibles having anchors

Family Cites Families (17)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US3640398A (en) * 1970-03-30 1972-02-08 Edward J Mellen Jr Wafer boat
JPS6369734A (ja) * 1986-09-10 1988-03-29 Fujitsu Ltd 光フアイバ固定方法
JPH0733305B2 (ja) * 1987-03-20 1995-04-12 三菱マテリアル株式会社 石英製二重ルツボの製造方法
JPH0633218B2 (ja) * 1987-12-08 1994-05-02 日本鋼管株式会社 シリコン単結晶の製造装置
JPH03177397A (ja) * 1989-12-04 1991-08-01 Agency Of Ind Science & Technol 有機化合物結晶の製造方法
US5284631A (en) * 1992-01-03 1994-02-08 Nkk Corporation Crucible for manufacturing single crystals
JP2830990B2 (ja) * 1995-05-31 1998-12-02 信越石英株式会社 石英製二重ルツボの製造方法
US5653777A (en) * 1995-10-19 1997-08-05 Uop Bonding procedure for silica assemblies
JP3769800B2 (ja) * 1996-01-12 2006-04-26 株式会社Sumco 単結晶引上装置
JP2003054971A (ja) * 2001-08-09 2003-02-26 Fujitsu Ltd 石英ガラスの接合方法
US7635414B2 (en) * 2003-11-03 2009-12-22 Solaicx, Inc. System for continuous growing of monocrystalline silicon
WO2006024440A1 (de) * 2004-08-28 2006-03-09 Heraeus Quarzglas Gmbh & Co. Kg Fügemittel zum verbinden von bauteilen, verfahren zum verbinden von bauteilen aus hochkieselsäurehaltigem werkstoff unter einsatz des fügemittels, sowie nach dem verfahren erhaltener bauteil-verbund
JP4867684B2 (ja) * 2007-02-01 2012-02-01 セイコーエプソン株式会社 光学部材の接合方法
US8262797B1 (en) * 2007-03-13 2012-09-11 Solaicx, Inc. Weir design providing optimal purge gas flow, melt control, and temperature stabilization for improved single crystal growth in a continuous Czochralski process
DE102007060980A1 (de) * 2007-12-14 2009-06-18 Heraeus Quarzglas Gmbh & Co. Kg Verfahren zum Verbinden von Bauteilen aus hochkieselsäurehaltigen Werkstoffen
JP5467653B2 (ja) * 2011-01-13 2014-04-09 信越石英株式会社 ガラス多角管及びその製造方法並びに容器
JP5741163B2 (ja) * 2011-04-11 2015-07-01 信越半導体株式会社 石英ガラスルツボ及びその製造方法、並びにシリコン単結晶の製造方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
None

Also Published As

Publication number Publication date
CN104870394A (zh) 2015-08-26
US20140174338A1 (en) 2014-06-26
WO2014100487A3 (en) 2015-03-05
JP2016505503A (ja) 2016-02-25

Similar Documents

Publication Publication Date Title
KR101467103B1 (ko) 실리콘 단결정 성장 장치 및 그 성장 방법
US20090249994A1 (en) Crystal growth apparatus and method
KR101901308B1 (ko) 실리콘 융액면의 높이위치의 산출방법 및 실리콘 단결정의 인상방법 그리고 실리콘 단결정 인상장치
US9863063B2 (en) Weir for inhibiting melt flow in a crucible
US20170356099A1 (en) Apparatus and method for introducing volatile dopants into a melt
EP2510138B1 (en) Methods for manufacturing monocrystalline germanium ingots/wafers having low micro-pit density (mpd)
US20130263772A1 (en) Method and apparatus for controlling melt temperature in a Czochralski grower
JPWO2001063023A1 (ja) 半導体単結晶の成長方法
KR101596550B1 (ko) 잉곳성장장치 및 잉곳성장방법
US20140174338A1 (en) Methods to bond silica parts
CN108796603B (zh) 一种直拉单晶补掺合金的工艺方法
JP2019043788A (ja) 単結晶育成方法及び単結晶育成装置
EP2501844A1 (en) Crystal growth apparatus and method
JP7486743B2 (ja) FeGa合金単結晶の製造方法
TW202421861A (zh) 單晶爐及單晶矽的製備方法
JPS5930795A (ja) 単結晶引上装置
CN115558984B (zh) 一种无坩埚制备大尺寸半导体晶体的方法
CN218404490U (zh) 一种无坩埚制备大尺寸半导体晶体的装置
JPS59227797A (ja) 単結晶の引上げ方法
JP2009023867A (ja) 半導体結晶の製造方法及びその製造装置
JP7349100B2 (ja) FeGa単結晶育成用種結晶及びFeGa単結晶の製造方法
CN115537911A (zh) 提拉法制备大尺寸晶体的方法和设备
KR101339151B1 (ko) 단결정 실리콘 잉곳 제조 장치 및 방법
JPS6011297A (ja) 結晶育成制御方法及び制御装置
JPH111388A (ja) 単結晶成長方法及び装置

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 13818634

Country of ref document: EP

Kind code of ref document: A2

ENP Entry into the national phase

Ref document number: 2015549738

Country of ref document: JP

Kind code of ref document: A

122 Ep: pct application non-entry in european phase

Ref document number: 13818634

Country of ref document: EP

Kind code of ref document: A2