KR101529857B1 - Salt mortar composition for building materials - Google Patents

Salt mortar composition for building materials Download PDF

Info

Publication number
KR101529857B1
KR101529857B1 KR1020150039838A KR20150039838A KR101529857B1 KR 101529857 B1 KR101529857 B1 KR 101529857B1 KR 1020150039838 A KR1020150039838 A KR 1020150039838A KR 20150039838 A KR20150039838 A KR 20150039838A KR 101529857 B1 KR101529857 B1 KR 101529857B1
Authority
KR
South Korea
Prior art keywords
salt
extract
mortar composition
mortar
present
Prior art date
Application number
KR1020150039838A
Other languages
Korean (ko)
Inventor
박종범
Original Assignee
대복건설 주식회사
박종범
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 대복건설 주식회사, 박종범 filed Critical 대복건설 주식회사
Priority to KR1020150039838A priority Critical patent/KR101529857B1/en
Application granted granted Critical
Publication of KR101529857B1 publication Critical patent/KR101529857B1/en

Abstract

The present invention relates to a salt mortar composition for a building material, and more specifically, to a salt mortar composition which is made of natural materials only which are beneficial to a human body, and has an adhesive strength, crack resistance, water resistance, etc. required for a mortar for gluing a thing such as a tile, a wall body, a floor material or the like. According to the present invention, the salt mortar composition for a building material includes functions such as far-infrared radiation emission, deodorization, etc. like red clay or a white clay stone, and satisfies the adhesive strength, the crack resistance, the water resistance, etc. required for the mortar for building gluing. Therefore, the present invention enables to be constructed on a partition, cement, a wall paper, a plaster board, etc., and has an effect on an atopy amelioration, a blood circulation function, a fatigue recovery, a respiratory disease treatment, etc. as being made of natural materials only, which enable to produce the large amount of an anion. In addition, by using eco-friendly materials only replacing a chemical material causing an environment pollution such as cement, the present invention enables to contribute to prevent the environment pollution.

Description

건축 자재용 소금 모르타르 조성물{Salt mortar composition for building materials}[0001] Salt mortar composition for building materials [

본 발명은 건축 자재용 소금 모르타르 조성물에 관한 것으로, 더욱 구체적으로는 인체에 유익한 천연 재료만으로 이루어지면서도 타일, 벽체 또는 바닥재 등의 접착용 모르타르에 요구되는 접착강도, 내균열성, 내수성 등을 구비한 건축 자재용 소금 모르타르 조성물에 관한 것이다. The present invention relates to a salt mortar composition for building materials, and more particularly to a salt mortar composition for building materials, which is composed of only natural materials beneficial to the human body and has adhesion strength, crack resistance and water resistance required for adhesive mortar such as tile, To a salt mortar composition for a building material.

일반적으로, 모르타르(mortar)라 함은 시멘트와 모래의 혼합물을 일컫는데, 이것은 콘크리트와 동일한 부위에 물과 함께 혼합되어 이의 경화 작용에 의하여 접착제의 성질을 지니게 된다. 이러한 모르타르는 석회, 아스팔트, 합성수지 등의 고착제를 포함할 수 있고, 포함된 고착제의 종류에 따라 석회 모르타르, 아스팔트 모르타르, 수지 모르타르, 질석 모르타르, 펄라이트 모르타르 등으로 구분될 수 있으며, 벽, 바닥, 천장 바탕 등의 마감 재료로도 활용된다. 비교적 값싼 재료인 반면에 강도, 내화성, 내수성, 내구성 등이 우수하여 건축을 비롯한 건설공사 전반에 걸쳐 광범위하게 사용되고 있다.Generally, mortar refers to a mixture of cement and sand, which is mixed with water at the same site as concrete and has adhesive properties due to its hardening action. Such mortar may include a fixing agent such as lime, asphalt, and synthetic resin, and may be classified into lime mortar, asphalt mortar, resin mortar, vermiculite mortar, and pearlite mortar depending on the type of the fixing agent. It is also used as a finishing material for the base. It is a relatively inexpensive material, but has excellent strength, fire resistance, water resistance and durability and is widely used throughout construction and other construction works.

특히, 건조 시멘트 모르타르는 공동주택 및 공공주택의 마감을 구성하는 주요 건축 재료로서, 사람과 가장 밀접하게 접촉하는 생활공간의 주요부를 구성하는 재료인데, 포장된 시멘트 및 포장되어 완전히 건조된 모래를 현장에서 물을 일정량 첨가하여 사용된다.In particular, dry cement mortar is the main building material that constitutes the finish of apartment houses and public houses. It constitutes the main part of the living space which is in closest contact with people. It is composed of packed cement and packed, Is added by adding a certain amount of water.

이와 같이, 종래의 건조 시멘트 모르타르는 크게 시멘트와 골재, 사용수 및 혼합재료로 구성되는 복합재료로서, 지금까지 대부분 구조체의 내구성 확보 및 시멘트 경화에 따라 발생되는 건조수축에 의한 균열을 방지하는 부분에 대하여 중점적으로 제공되었으나 환경에 대한 부분은 검토되지 않았거나, 혹은 맥반석이나 장석 등을 골재로 이용하여 제조된 것으로 다양한 기능 중 제한적인 기능만을 부여한 제품만이 유통되고 있는 실정이다.As described above, conventional dry cement mortar is a composite material composed largely of cement, aggregate, used water and mixed material. In the past, most parts to prevent durability of the structure and crack due to drying shrinkage caused by cement hardening However, the environment has not been reviewed, or only products that have been manufactured using the elvan stone or feldspar as aggregate have been given only limited functions among various functions.

그 결과, 건조 시멘트 모르타르에 포함된 대표적인 무기결합제인 시멘트를 제조하는 공정 중에 주성분인 CaCO3의 열처리 과정에서 막대한 양의 에너지(약 30~35ℓ/ton)가 소비되며, 시멘트 1톤 제조 시 석회석과 규산의 화학 반응만으로도 약 800kg의 이산화탄소가 배출되는 것으로 알려져 있을 뿐만 아니라, 시멘트에 포함된 각종 환경 오염원으로 인하여 아토피성피부염, 천식, 새집증후군 등과 같은 증상이 유발되는 등 환경성 질환의 원인이 되고 있으며, 강알칼리성으로 인하여 식생물의 생육을 심각하게 저하시키는 문제점이 있다.As a result, a large amount of energy (about 30 ~ 35 L / ton) is consumed in the heat treatment process of the main component CaCO 3 during the process of manufacturing cement, which is a typical inorganic binder in dry cement mortar, It is known that only about 800 kg of carbon dioxide is emitted by the chemical reaction of silicic acid. In addition, due to various environmental pollutants contained in the cement, environmental diseases such as atopic dermatitis, asthma and sick house syndrome are caused. There is a problem that the growth of food organisms is severely lowered due to the strong alkalinity.

또한, 건조 모르타르는 모래에 수분이 없어 유동성이 현저히 떨어진다. 이를 방지하기 위하여 일반적으로 분말형의 화학 감수제를 첨가하는데, 이 감수제는 환경오염의 원인이 된다. 이에 따라, 상술된 문제점이 해결된 새로운 조성의 친환경 모르타르에 대한 개발 필요성이 대두되고 있는 실정이다.In addition, the dry mortar has a considerable deterioration in fluidity due to lack of moisture in the sand. To prevent this, a powdery chemical reducing agent is generally added, which causes environmental pollution. Accordingly, there is a growing need for the development of eco-friendly mortar having the above-mentioned problems and solving the above-mentioned problems.

한국 등록특허 제10-0614451호(2006.08.14.)Korean Patent No. 10-0614451 (2006.08.14.) 한국 등록특허 제10-0986790호(2010.10.04.)Korean Patent No. 10-0986790 (Apr. 4, 2010)

본 발명은 상기와 같은 문제점을 해소하고자 안출(案出)된 것으로서, 본 발명의 목적은 친환경적이고 인체에 유익한 성분을 다량 방출하면서도 건축용 모르타르에 요구되는 접착강도, 내균열성, 내수성 등을 충족시킬 수 있는 건축 자재용 소금 모르타르 조성물을 제공하는데에 있다.It is an object of the present invention to solve the above-mentioned problems, and it is an object of the present invention to provide a mortar composition which is capable of satisfying adhesive strength, cracking resistance, water resistance and the like required for a mortar for construction while releasing a large amount of environmentally- And to provide a salt mortar composition for building materials.

이러한 목적을 달성하기 위한 본 발명에 따른 건축 자재용 소금 모르타르 조성물은,In order to accomplish the above object, the present invention provides a salt mortar composition for building materials,

녹말 12.5~15.0중량%, 설탕 6.5~11.5중량%, 다시마 추출물 12.5~17.5중량%, 찹쌀발아 7.5~12.5중량%, 솔잎 추출물 12.5~17.5중량%, 은행나무 추출물 2.5~5.0중량% 및 물 17.0~22.0중량%로 혼합되어 구성된 천연 혼합 추출물;A ginseng extract 12.5 to 17.5 wt.%, A glutinous rice germination 7.5 to 12.5 wt.%, A pine needle extract 12.5 to 17.5 wt.%, A ginkgo extract 2.5 to 5.0 wt.% And a water 17.0 to 15.0 wt. 22.0% by weight of a natural mixed extract;

상기 천연 혼합 추출물 19.0~21.4중량%, 소금 70~75중량% 및 허브 오일 6~10중량%로 혼합하여 이루어지는 것을 특징으로 한다.The natural mixed extract is mixed in an amount of 19.0 to 21.4% by weight, 70 to 75% by weight of salt and 6 to 10% by weight of herbal oil.

또한, 상기 허브 오일은 라벤더, 로즈마리, 민트, 구본초, 쑥, 솔잎으로 이루어진 군으로부터 선택되는 하나 이상의 혼합물로 이루어지는 것을 특징으로 한다.The herbal oil is characterized in that the herbal oil is composed of at least one selected from the group consisting of lavender, rosemary, mint, syrup, wormwood, pine leaf.

또한, 상기 천연 혼합 추출물 및 이 천연 혼합 추출물과 소금 및 허브 오일의 혼합은 교반기에 의해서 30분 내지 60분 동안 300rpm 내지 900rpm의 교반 속도로 교반시켜 이루어지는 것을 특징으로 한다.In addition, the natural mixed extract, the natural mixed extract, the salt and the herbal oil are mixed by stirring with a stirrer at 300 rpm to 900 rpm for 30 minutes to 60 minutes.

그리고, 상기 천연 혼합 추출물은 4일 내지 7일간 상온에서 숙성시켜 액상으로 형성되는 것을 특징으로 한다.The natural mixed extract is characterized by being formed into a liquid phase by aging at room temperature for 4 days to 7 days.

아울러, 상기 소금은 800℃ 내지 1,000℃에서 8시간 구운 천일염으로 이루어지는 것을 특징으로 한다.In addition, the salt is characterized in that the salt is formed of the sun-dried salt baked at 800 ° C to 1,000 ° C for 8 hours.

한편, 상기 조성물은 전단 접착 강도가 0.40N/㎟ 내지 0.60N/㎟ 으로서, 파티션, 시멘트, 벽지 및 석고보드에 시공되는 것을 특징으로 한다.On the other hand, the composition has a shear bond strength of 0.40 N / mm < 2 > to 0.60 N / mm < 2 >, and is applied to partitions, cement, wallpaper and gypsum board.

다른 한편, 상기 조성물은 식용색소, 분말도료, 황토, 백토석 및 안료제의 군에서 선택되는 하나 이상의 추가의 성분을 포함하여 다양한 색상을 발현시키는 것을 특징으로 한다.On the other hand, the composition is characterized by expressing various colors including one or more additional components selected from the group of food colors, powder paints, loess, white peach and pigment.

또한, 상기 천연 혼합 추출물은 증점제 성분을 추가로 혼합하여 접착력이 증대되는 것을 특징으로 한다.Further, the natural mixed extract is characterized in that the adhesive strength is increased by further mixing the thickener component.

아울러, 상기 소금 모르타르 조성물은 접착 시 서서히 굳어지면서 용해된 소금이 상온에서 재결정화되는 과정을 포함하여 이루어지는 것을 특징으로 한다.In addition, the salt mortar composition is characterized in that the salt is gradually hardened at the time of bonding and the dissolved salt is recrystallized at room temperature.

본 발명에 따른 건축 자재용 소금 모르타르 조성물은 황토 또는 백토석과 같이 원적외선 방출, 탈취 등의 기능을 포함하고, 건축 접착용 모르타르에 요구되는 접착강도, 내균열성, 내수성 등을 충족함으로서 파티션, 시멘트, 벽지 및 석고보드 등에 시공이 가능하며, 음이온을 다량 발산시킬 수 있는 천연 재료만으로 이루어져 아토피 개선, 혈액의 순환 작용, 피로회복, 호흡기 질환 치유 등에 탁월한 효과가 있다. 또한, 시멘트 등의 환경오염을 유발할 수 있는 화학물질을 대체하여 친환경적인 재료만을 사용함으로써, 환경오염 방지에도 기여할 수 있다.The salt mortar composition for building materials according to the present invention includes functions of releasing and deodorizing far-infrared rays such as yellow clay and white clay, and satisfies the adhesive strength, crack resistance and water resistance required for construction adhesive mortar, It can be applied to wallpaper, gypsum board, etc. It is made of only natural materials that can dissolve a large amount of anions, and has excellent effects on improvement of atopy, circulation of blood, restoration of fatigue, and healing of respiratory diseases. In addition, by using only eco-friendly materials in place of chemical substances that can cause environmental pollution such as cement, it can contribute to prevention of environmental pollution.

도 1은 본 발명의 바람직한 일 실시예에 따른 소금 모르타르 조성물을 나타낸 사진이다.
도 2는 본 발명의 바람직한 일 실시예에 따른 천연 혼합 추출물을 나타낸 사진이다.
도 3은 본 발명의 바람직한 일 실시예에 따른 천연 혼합 추출물에 소금이 첨가되는 상태를 나타낸 사진이다.
도 4는 본 발명의 바람직한 일 실시예에 따른 천연 혼합 추출물과 소금이 혼합된 상태에서 허브 오일을 첨가시키는 사진이다.
도 5 내지 도 7은 본 발명의 바람직한 일 실시예에 따른 소금 모르타르 조성물을 이용한 시공 사진이다.
도 8은 본 발명의 바람직한 일 실시예에 따른 소금 모르타르를 이용한 벽체 시공 완료 사진이다.
1 is a photograph showing a salt mortar composition according to a preferred embodiment of the present invention.
2 is a photograph showing a natural mixed extract according to a preferred embodiment of the present invention.
3 is a photograph showing a state where salt is added to a natural mixed extract according to a preferred embodiment of the present invention.
FIG. 4 is a photograph showing the addition of herbal oil in a state where a natural mixture extract and salt are mixed according to a preferred embodiment of the present invention.
5 to 7 are photographs of a construction using a salt mortar composition according to a preferred embodiment of the present invention.
FIG. 8 is a photograph showing completion of a wall construction using a salt mortar according to a preferred embodiment of the present invention.

본 발명은 일면에 있어서,In one aspect of the present invention,

녹말 12.5~15.0중량%, 설탕 6.5~11.5중량%, 다시마 추출물 12.5~17.5중량%, 찹쌀발아 7.5~12.5중량%, 솔잎 추출물 12.5~17.5중량%, 은행나무 추출물 2.5~5.0중량% 및 물 17.0~22.0중량%로 혼합되어 구성된 천연 혼합 추출물;A ginseng extract 12.5 to 17.5 wt.%, A glutinous rice germination 7.5 to 12.5 wt.%, A pine needle extract 12.5 to 17.5 wt.%, A ginkgo extract 2.5 to 5.0 wt.% And a water 17.0 to 15.0 wt. 22.0% by weight of a natural mixed extract;

상기 천연 혼합 추출물 19.0~21.4중량%, 소금 70~75중량% 및 허브 오일 6~10중량%로 혼합하여 이루어지는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물을 제공한다.Wherein the natural mixed extract is mixed with 19.0 to 21.4 wt%, 70 to 75 wt% of salt and 6 to 10 wt% of herbal oil.

이하, 본 발명의 바람직한 실시예에 대하여 상세하게 설명한다.Hereinafter, preferred embodiments of the present invention will be described in detail.

이에 앞서, 본 명세서 및 특허청구범위에 사용된 단어는 통상적이거나 사전적인 의미로 한정 해석하지 아니하며, 발명자는 그 자신의 발명을 가장 최선의 방법으로 설명하기 위해 용어의 개념을 적절하게 정의할 수 있다는 원칙에 입각하여 본 발명의 기술적 사상에 부합하는 의미와 개념으로 해석되어야만 한다.Prior to this, words used in this specification and claims are not to be construed in a conventional or dictionary sense, and the inventor can appropriately define the concept of a term to describe its own invention in the best way And should be construed in accordance with the principles and meanings and concepts consistent with the technical idea of the present invention.

본 발명에 따른 소금 모르타르 조성물은 4일 내지 7일 동안 상온에서 숙성시킨 천연 혼합 추출물과 소금 및 허브 오일을 혼합하여 이루어진다.The salt mortar composition according to the present invention is prepared by mixing a natural mixed extract aged at room temperature for 4 to 7 days with salt and herb oil.

상기 천연 혼합 추출물은 녹말 12.5 내지 15.0중량%, 설탕 6.5 내지 11.5중량%, 다시마 추출물 12.5 내지 17.5중량%, 찹쌀발아 7.5 내지 12.5중량%, 솔잎 추출물 12.5 내지 17.5중량%, 은행나무 추출물 2.5 내지 5.0중량% 및 물 17.0 내지 22.0중량%를 교반시켜 상온에서 4일 내지 7일 동안 숙성시키면, 도 2에 첨부된 사진에서 보이는 바와 같이, 묽은 색상의 무른 물성을 지니는 액상으로 이루어질 수 있다. 이때, 상기 교반은 교반기에 의해서 30분 내지 60분 동안 300rpm 내지 900rpm의 교반 속도로 이루어짐이 바람직하다.The natural mixture extract contains 12.5 to 15.0 wt% of starch, 6.5 to 11.5 wt% of sugar, 12.5 to 17.5 wt% of seaweed extract, 7.5 to 12.5 wt% of glutinous rice germination, 12.5 to 17.5 wt% of pine needle extract, 2.5 to 5.0 wt. % Of water and 17.0 to 22.0% by weight of water are agitated at room temperature for 4 days to 7 days. As shown in the photograph attached to FIG. 2, the liquid phase may have a weak color property. At this time, it is preferable that the stirring is performed by a stirrer at a stirring speed of 300 rpm to 900 rpm for 30 minutes to 60 minutes.

추가로, 조성물의 접착력이 배가되도록 증점제 성분을 혼합할 수도 있다. 상기 증점제는 점성 또는 점탄성을 임의로 조정하는 성분으로써, 목적에 적절한 점성 및 점탄성의 효과를 기대할 수 있다.In addition, the thickener component may be mixed so that the adhesion of the composition is doubled. The thickening agent is a component that arbitrarily adjusts the viscosity or viscoelasticity, and the effect of viscosity and viscoelasticity suitable for the purpose can be expected.

한편, 상기와 같이 혼합되어 교반된 천연 혼합 추출물은, 상기 천연 혼합 추출물 19.0 내지 21.4중량%에 소금 70 내지 75중량%와 허브 오일 6 내지 10중량%를 교반시키면 소금 모르타르 조성물을 얻을 수 있다. 상기와 같은 혼합비로 얻어진 소금 모르타르는 흰색의 무른 물성으로 형성되며, 강한 접착 성질을 지닐 수 있는데, 이때, 접착 강도는 0.40N/㎟ 내지 0.60N/㎟ 이다. 물론, 혼합되는 원료의 배합비에 따라 상기 접착 강도는 변경될 수 있음은 자명하다. 또한, 상기 천연 혼합 추출물에 황토 분말과 숯 분말을 추가로 혼합시킨 소금 모르타르 조성물을 마감재로 사용하면, 실내에 습기를 머금었다가 다시 건조되는 현상을 반복하는 자연가습기 역할을 수행할 수 있다.Meanwhile, the natural mixed extract may be prepared by stirring 70 to 75% by weight of salt and 6 to 10% by weight of herbal oil in 19.0 to 21.4% by weight of the natural mixed extract. The salt mortar obtained in the mixing ratio as described above is formed into a whitish soft property and can have strong adhesive properties, wherein the adhesive strength is 0.40 N / mm 2 to 0.60 N / mm 2. It goes without saying that the above adhesive strength can be changed depending on the blending ratio of the raw materials to be mixed. In addition, when the salt mortar composition in which the natural mixed extract is further blended with the loess powder and the char powder is used as the finishing material, the natural humidifier can function as a natural humidifier repeatedly drying the moisture in the room and drying it again.

상기 소금 모르타르 조성물은 혼합되어 첨가되는 소금의 입자 크기에 따라서 질감이 달리 나타날 수 있는데, 이는 상기 소금 모르타르 조성물이 벽체 또는 바닥재 등에 접착 시 서서히 굳어지면서 용해되어진 소금이 상온에서 재결정화되는 과정을 포함하기 때문이다.The salt mortar composition may be different in texture depending on the particle size of the salt added to the salt mortar composition. The salt mortar composition may include a process of recrystallizing the dissolved salt at room temperature when the salt mortar composition is solidified when the salt mortar composition is adhered to a wall or a floor material. Because.

따라서, 소금의 입자 크기가 작으면 무른 물성의 질감이 나타나고, 소금의 입자 크기가 크면 거친 물성의 질감을 나타낼 수 있다.Therefore, when the particle size of the salt is small, the texture of the physical property appears, and when the particle size of the salt is large, the texture of the rough property can be exhibited.

한편, 상기 소금은 800℃ 내지 1,000℃에서 8시간 구운 천일염을 사용하는게 바람직하나, 이와 동등한 성분인 정제염을 사용할 수도 있다.On the other hand, it is preferable that the salt is baked at 800 ° C to 1,000 ° C for 8 hours, but a purified salt equivalent to the salt may also be used.

별법으로, 상기 소금 모르타르 조성물을 얻기 위해 혼합물을 교반시킬 때, 식용색소, 분말도료, 황토, 백토석 및 안료제의 군에서 선택되는 하나 이상의 추가 성분을 소량 혼합하면 조성물에 다양한 색상을 발현시킬 수 있다.Alternatively, mixing a small amount of one or more additional ingredients selected from the group of edible pigments, powder coatings, loess, white pebbles and pigments with stirring to obtain the salt mortar composition can result in a variety of colors being expressed in the composition have.

상기 천연 혼합 추출물은 녹말이 12.5중량% 미만이고, 설탕이 11.5중량%를 초과하면 접착강도와 내수성이 약화되고, 반대로 녹말의 비율이 15.0중량%를 초과하고, 설탕이 6.5% 미만이면 점도가 높아져 작업성 측면에서 효율적이지 못하다.When the proportion of starch is more than 15.0 wt% and sugar is less than 6.5 wt%, the viscosity of the natural mixed extract is increased. It is not efficient in terms of workability.

상기 다시마 추출물은 일정한 점성을 지니는 특성이 있으므로, 혼합물과 교반되어 형성된 소금 모르타르 조성물의 접착력을 증대시킬 수 있으며, 또한, 천연 성분이므로 인체에 유익할 수 있다. 상기 다시마 추출물은 12.5중량% 미만이면 점성 기능이 약화되고, 17.5중량%를 초과하면 점성 기능의 상승 작용이 나타나지 않으므로 경제적이지 못하다. Since the kelp extract has a certain viscosity, it can increase the adhesive strength of the salt mortar composition formed by stirring with the mixture, and can be beneficial to the human body because it is a natural ingredient. If the content of the sea tangle extract is less than 12.5% by weight, the viscous function is weakened. If the content is more than 17.5% by weight, syneresis of the viscous function is not exhibited.

상기 찹쌀발아는 아밀로펙틴이 주성분으로 이루어지는데, 상기 아밀로펙틴은 끈적거리는 성분으로 이루어지면서 강하게 달라붙는 성질이 있다. 상기 찹쌀발아는 7.5중량% 미만이면 달라붙는 성질이 약화되며, 12.5중량%를 초과하면 달라붙는 성질이 강해지면서 모르타르가 굳어지는 현상이 나타나므로 기능성 측면에서 가치가 급격하게 하락하게 된다.The glutinous rice germination is mainly composed of amylopectin. The amylopectin has sticky components and sticks strongly. If the glutinous rice germination is less than 7.5% by weight, the sticking property is weakened. If the glutinous rice germination exceeds 12.5% by weight, the sticking property is strengthened and the hardening of the mortar occurs.

상기 솔잎 추출물은 a-pinene, β-pinene, camphene 등으로 조성된 terpenes과 같은 정유 성분과 폴리페놀(polyphenol), 폴라보노이드(flavonoid)류, 무기 및 유기성분, 비타민류 등 다양한 성분이 함유되어 있는데, 이 중 terpenes 성분은 곰팡이 및 세균 등의 성장을 저해하는 효과를 나타내고, 또한, 솔잎 추출물의 성분 중에는 폴리페놀(polyphenol) 성분인 수용성 탄닌의 함량이 높은데, 이 탄닌은 항균 작용 및 항바이러스 작용과 항산화능, 부패성 미생물 생육 저해능이 있을 수 있다. 따라서, 건물 건축 시, 상기 솔잎 추출물이 포함된 소금 모르타르 조성물로 벽지 등을 시공할 때, 유해한 성분이 제거됨으로써, 새집증후군과 같은 현상을 억제할 수 있는 효과가 있다.The pine needle extract contains various components such as essential oils such as terpenes such as a-pinene, p-pinene and camphene, polyphenol, flavonoid, inorganic and organic components and vitamins. Among them, terpenes have the effect of inhibiting the growth of fungi and bacteria. In addition, the component of pine leaf extract has a high content of water-soluble tannin, which is a polyphenol component. The tannin has antimicrobial activity and antiviral activity And antioxidant ability, and may inhibit the growth of pernicious microorganisms. Accordingly, when a wall or the like is applied to a salt mortar composition containing the pine leaf extract at the time of building construction, harmful components are removed, thereby suppressing phenomena such as sick house syndrome.

또한, 은행나무 추출물은 수피로부터 추출된 추출물로, 유효 성분으로 포함하는 항균물질을 제공할 수 있으며, 상기 은행나무 추출물을 소금 모르타르 조성물을 제조하기 위한 혼합물에 첨가함으로써 항균 효과를 제공받을 수 있다. 또한, 부패 방지 또는 선도 유지뿐만 아니라 항균제, 항미생물제 등 항균력을 발휘하는 성분으로 매우 유용하게 사용될 수 있다.Also, the ginkgo extract may be an extract extracted from bark, and may provide an antimicrobial substance contained as an active ingredient. The antimicrobial effect may be provided by adding the ginkgo extract to a mixture for preparing a salt mortar composition. In addition, it can be very usefully used as a component that exhibits antimicrobial activity such as antimicrobial agent, antimicrobial agent, as well as prevention of corruption or maintenance of leading.

상기 천연 혼합 추출물의 혼합에 있어서, 물을 첨가할 수 있는데 17.0중량% 미만이면, 점성은 높아지나 단시간 내에 굳어지며, 반대로 22.0중량%를 초과하면 점성이 낮아짐과 동시에 접착 강도가 현저히 떨어지게 된다.In the mixing of the natural mixed extract, water can be added. When the content is less than 17.0% by weight, the viscosity becomes high but hardens in a short time. On the other hand, when the content is more than 22.0% by weight, the viscosity decreases and the bonding strength remarkably decreases.

한편, 향기로운 향을 발산하여 사용자에게 심신의 안정감을 취할 수 있도록 허브 오일을 첨가할 수 있는데, 상기 허브 오일은 라벤더, 로즈마리, 민트, 구본초, 쑥, 솔잎으로 이루어진 군으로부터 선택되는 하나 이상의 혼합물로 이루어질 수 있으며, 특히, 허브 오일은 효모의 생육을 강하게 억제함은 물론, 타 혼합물과 동시에 혼합되는 재료로서, 사용 시 더욱 광범위하게 항균성 및 항진균성의 성질을 나타낸다. 또한, 향기로운 향을 발산하여 사용자에게 마음의 안정감을 취할 수 있도록 할 수 있다.On the other hand, it is possible to add herbal oil so as to radiate fragrant fragrance to the user so as to take a sense of mind and body stability. The herbal oil is at least one compound selected from the group consisting of lavender, rosemary, mint, In particular, herb oil is a material which strongly inhibits the growth of yeast and is mixed with other mixture at the same time, and exhibits antibacterial and antifungal properties more widely when it is used. In addition, it is possible to emit a fragrant fragrance so that the user can feel a sense of security of mind.

따라서, 상기 허브 오일을 소금 모르타르 조성물 제조 시 혼합함으로서, 전술한 항균성, 항진균성 및 향기 등의 효과를 얻는데 더욱 유리할 수 있다. 한편, 상기한 성분을 대신하여 동등한 기능을 수행하는 재료이면 대체하여 사용이 가능할 수 있다.Therefore, by mixing the herb oil during the production of the salt mortar composition, it may be more advantageous to obtain the above-mentioned effects such as antimicrobial activity, antifungal activity and aroma. On the other hand, a material that performs the equivalent function instead of the above-described components may be used in place of the above-mentioned components.

이와 같은 본 발명에 따른 건축 자재용 소금 모르타르 조성물은 강한 접착력을 지닌 무른 물성으로 형성되고, 전단 접착 강도가 0.40N/㎟ 내지 0.60N/㎟ 으로서 접착강도가 매우 우수할 뿐만 아니라, 내균열성, 내수성은 물론, 항균 효과로 새집증후군과 같은 유해 환경을 제거할 수 있고, 음이온을 다량 발산시킬 수 있는 천연 재료만으로 이루어져 아토피 개선, 혈액의 순환 작용, 피로회복, 호흡기 질환 치유 등에 탁월한 효과가 있다. The salt mortar composition for building material according to the present invention is formed into a soft material having strong adhesive force and has a shear bond strength of 0.40 N / mm 2 to 0.60 N / mm 2, and has excellent adhesive strength, It is not only water resistant but also has an antimicrobial effect that can remove harmful environment such as sick house syndrome and is made of only natural materials capable of emitting a large amount of anion, and thus has an excellent effect on improvement of atopy, circulation of blood, restoration of fatigue and healing of respiratory diseases.

하기에서는, 본 발명에 따른 건축 자재용 모르타르 조성물의 실시예 및 실험예에 대하여 설명한다. 그러나, 이들 실시예 및 실험예는 본 발명의 이해를 돕기 위해 기술한 것으로서 발명의 내용 및 범위를 제한하지 않는다.Hereinafter, examples and experimental examples of the mortar composition for building materials according to the present invention will be described. However, these examples and experimental examples are described for the purpose of helping understanding of the present invention, and do not limit the content and scope of the invention.

하기 실험은 공인 시험 기관(화학시험연구원)에 의뢰하여 통상적인 시험 평가 기준에 의거하여 실시하였다.
The following experiment was carried out according to a standard test evaluation standard by an authorized testing institute (Chemical Test Research Institute).

(( 실시예Example 1) One)

통상의 교반기를 사용하여, 하기 표 1에 나타난 비율로 각 성분을 30분간 500rpm의 속도로 교반시켜 천연 혼합 추출물을 제조하였다.
Each component was stirred for 30 minutes at a speed of 500 rpm using a conventional stirrer at the ratios shown in Table 1 below to prepare a natural mixed extract.

조 성Furtherance 함 량(g)Content (g) 녹말starch 3030 설탕Sugar 4040 다시마 추출물Seaweed extract 3030 찹쌀발아Glutinous rice germination 1818 솔잎 추출물Pine leaf extract 3030 은행나무 추출물Ginkgo extract 66 water 4040

상기 표 1과 같이 교반되어 제조되어진 천연 혼합 추출물을 하기 표2에 나타난 비율로 각 성분을 30분간 500rpm의 속도로 교반시켜 소금 모르타르 조성물을 제조하였다.
The natural mixed extracts prepared as described in Table 1 were stirred at a rate of 500 rpm for 30 minutes at a rate shown in Table 2 below to prepare a salt mortar composition.

조 성Furtherance 함 량(g)Content (g) 천연 혼합 추출물Natural mixed extract 194194 소금Salt 800800 허브 오일Herbal oil 66

(( 실시예Example 2) 2)

통상의 교반기를 사용하여 하기 표 3에 나타난 비율로 각 성분을 30분간 500rpm의 속도로 교반시켜 천연 혼합 추출물을 제조하였다.
Each component was stirred for 30 minutes at a speed of 500 rpm using a conventional stirrer at the ratios shown in Table 3 below to prepare a natural mixed extract.

조 성Furtherance 함 량(g)Content (g) 녹말starch 2828 설탕Sugar 3535 다시마 추출물Seaweed extract 2525 찹쌀발아Glutinous rice germination 1616 솔잎 추출물Pine leaf extract 2525 은행나무 추출물Ginkgo extract 55 water 4040

상기 표 3과 같이 교반되어 제조되어진 천연 혼합 추출물을 하기 표 4에 나타난 비율로 각 성분을 30분간 500rpm의 속도로 교반시켜 소금 모르타르 조성물을 제조하였다.
The natural mixed extracts prepared by stirring as shown in Table 3 were stirred at a rate of 500 rpm for 30 minutes at the ratios shown in Table 4 below to prepare a salt mortar composition.

조 성Furtherance 함 량(g)Content (g) 천연 혼합 추출물Natural mixed extract 174174 소금Salt 700700 허브 오일Herbal oil 44

(( 실험예Experimental Example 1) 전단 접착 강도 시험 1) Shear bond strength test

'KS L 1592: 2005 시험방법'에 따라 소금 모르타르 조성물을 준비한 후, 크기 100mm×100mm의 도자기질 모자이크 타일을 부착한 시험 샘플을 준비하였다. 상기 시험 샘플은 온도 23±2℃, 습도 50±5%의 항온 항습기에 6시간 저장 후에 전단 접착 강도 시험 샘플을 지지 기구에 결합시킨 후 9.8N/min의 속도로 하중을 인가하여 시험기가 나타내는 최대 하중을 구하고, 그 최대 하중을 타일 접착 면적으로 나누어 전단 접착 강도(N/㎟)를 측정하였다. 하기 표 5에 나타난 바와 같이, 전단 접착 강도는 각각 0.50이상, 0.45이상으로서, KS L 1592의 품질 기준에 부합하였다.
A salt mortar composition was prepared according to 'KS L 1592: 2005 Test Method', and then a test sample having a porcelain mosaic tile of size 100 mm x 100 mm was prepared. The test sample was stored for 6 hours in a thermostatic chamber at a temperature of 23 ± 2 ° C and a humidity of 50 ± 5%. After the sample was bonded to the support, the load was applied at a rate of 9.8 N / min. The load was determined, and the maximum load was divided by the tile adhesion area to determine the shear bond strength (N / mm 2). As shown in the following Table 5, the shear bond strengths were 0.50 or more and 0.45 or more, respectively, and met the quality standard of KS L 1592.

(( 실험예Experimental Example 2) 길이 변화율 시험 2) Length change rate test

상기 전단 접착 강도 시험에서와 동일한 방법으로 소금 모르타르 조성물을 준비하였다. 상기 모르타르 조성물을 KS L 5107의 규정에 따른 틀을 이용하여 시험 샘플을 준비한 후, 틀과 함께 약 72시간 동안 온도 23±2℃, 상대습도 95% 이상의 습기실에 저장하였다. 저장 기간 후에 틀을 분해하여 길이 측정용 콤퍼레이터를 이용하여 길이(L1)를 0.1mm까지 측정한 후, 온도 23±2℃, 습도 50±5%인 항온 항습기에 넣어 7일 경과 후 시험 샘플의 길이(L2)를 0.1mm까지 측정한 후, 하기 수식 1에 의해 길이 변화율(%)을 측정하였다.
A salt mortar composition was prepared in the same manner as in the above shear bond strength test. The mortar composition was prepared using a frame according to KS L 5107 and stored in a moisture chamber at a temperature of 23 ± 2 ° C. and a relative humidity of 95% for about 72 hours together with the frame. After the storage period, the frame was disassembled and the length (L1) was measured to a length of 0.1 mm using a length measuring comparator. The length of the test sample after 7 days was put into a thermo-hygrostat having a temperature of 23 ± 2 ° C. and a humidity of 50 ± 5% (L2) was measured up to 0.1 mm, and the rate of change in length (%) was measured according to the following equation (1).

Figure 112015027951622-pat00001
(수식 1)
Figure 112015027951622-pat00001
(Equation 1)

하기 표 5에 나타난 바와 같이, 길이 변화율은 각각 0.13이하, 0.15이하로서, KS L 1592의 품질 기준에 부합하였다.
As shown in Table 5 below, the rate of change in length was 0.13 or less and 0.15 or less, respectively, which satisfied the quality standard of KS L 1592.

(( 실험예Experimental Example 3) 보수율 시험 3) Conservation rate test

유리판 상부에 거름종이를 올려놓고 그 가운데 도우넛 형상의 틀을 설치한 후, 시료의 총질량 30%의 물을 첨가하고, 교반되어진 소금 모르타르 조성물을 주걱으로 도우넛 형상의 틀 내부에 채워 형틀의 높이와 수평이 일치되도록 초과되는 부분은 제거한 뒤, 즉시 그 상부에 유리판을 덮어 상하로 반복하여 뒤집어 준 후, 거름종이가 있는 부분이 위로 올라오도록 하였다. 측정은 약 60분 후에 거름종이가 배인 수분의 가장 큰 부분을 버니어캘리퍼스로 측정하고, 이의 직각 방향 구분의 크기를 0.1mm까지 측정하였고, 계산식은 하기 수식 2와 같다.
The dough paper was placed on the top of the glass plate, a donut-shaped frame was installed thereon, water having a total mass of 30% was added, and the stirred salt mortar composition was filled into the donut-shaped frame with a spatula, Immediately after removing excess parts to match the level, the top of the glass plate was covered with a glass plate and turned upside down repeatedly. The measurement was carried out with a vernier caliper to measure the largest part of the water having passed through the filter paper after about 60 minutes, and the size of the division in the perpendicular direction was measured up to 0.1 mm.

Figure 112015027951622-pat00002
(수식 2)
Figure 112015027951622-pat00002
(Equation 2)

하기 표 5에 나타난 바와 같이, 보수율은 각각 89, 88로서, KS L 1592의 품질 기준에 부합하였다.
As shown in Table 5 below, the water retention ratios were 89 and 88, respectively, and met the quality standard of KS L 1592.

(( 실험예Experimental Example 4) 위치 교정도 시험 4) Position calibration test

상기 전단 접착 강도 시험에서와 동일한 방법으로 소금 모르타르 조성물을 준비하였다. 상기 모르타르를 30×30cm의 석고 보드 상부에 6×6mm 요철 흙손으로 바른 다음, 평균 두께가 3mm가 되도록 타일을 붙여 시험 샘플을 제조하여 항온 항습기에 수평으로 넣어 둔 다음, 20분 후에 항온 항습기에서 꺼내서 개방 시간 조정 기구를 사용하여 타일을 바탕과 타일 사이를 2mm의 두께로 유지한 채 직각으로 바른 다음, 다시 처음 상태로 환원시켰을 때, 타일 자체 무게에 의해 낙하되는지를 검사하였다.A salt mortar composition was prepared in the same manner as in the above shear bond strength test. The mortar was applied to the upper part of a 30 × 30 cm gypsum board with a 6 × 6 mm uneven trowel and then a test sample was prepared by attaching tiles so that the average thickness was 3 mm and placed horizontally in a thermo-hygrostat. The opening time adjustment mechanism was used to apply a tile at a right angle while maintaining a thickness of 2 mm between the base and the tile, and then checked whether the tile was dropped by the weight of the tile when it was reduced to the initial state.

하기 표 5에 나타난 바와 같이, 위치 교정도(mm)는 모두 20 이상으로서, KS L 1592 품질 기준에 부합하였다.
As shown in Table 5 below, the positional correction degrees (mm) were all above 20, which met the KS L 1592 quality standard.

(( 실험예Experimental Example 5) 개방 시간 시험 5) Open time test

시험 샘플은 항온 항습기에서 30분 동안 유지시키는 것을 제외하면, 상기 위치 교정도 시험에서와 동일한 방식으로 개방 시간 시험을 시행하였다.The open time test was carried out in the same manner as in the above location calibration test, except that the test sample was kept in a thermostat for 30 minutes.

하기 표 5에 나타난 바와 같이, 개방 시간(min)은 모두 30 이상으로서, KS L 1592의 품질 기준에 부합하였다.
As shown in Table 5 below, all the open times (min) were over 30 and met the quality standard of KS L 1592.

평가 항목Evaluation items 실시예 1Example 1 실시예 2Example 2 품질 기준
(KS L 1592)
Quality standards
(KS L 1592)
전단 접착 강도
(N/㎟)
Shear bond strength
(N / mm < 2 &
0.50 이상0.50 or more 0.45 이상0.45 or more 0.35 이상0.35 or more
길이 변화율(%)Length change rate (%) 0.13 이하0.13 or less 0.15 이하0.15 or less 0.20 이하0.20 or less 보수율Rate of coverage 8989 8888 80~9580 ~ 95 위치교정도(min)Position calibration (min) 21~25℃
21 ~ 25 ℃
20 이상20 or more 20 이상20 or more 20 이상20 or more
개방시간(min)Open time (min) 30 이상30 or more 30 이상30 or more 30 이상30 or more

상기와 같이, 본 발명의 실시예 및 실험예에 따른 건축 자재용 소금 모르타르 조성물은 다량의 소금을 함유함에도 모르타르 조성물에 요구되는 전단 접착 강도, 길이 변화율, 보수율, 위치 교정도 및 개방 시간이 일반 시멘트 모르타르의 품질 기준(KS L 1592)과 부합되거나 훨씬 상회하는 것을 알 수 있다. 따라서, 타일이나 바닥재의 접착용에 적합하게 사용될 수 있다는 결론을 도출할 수 있다.As described above, although the salt mortar composition for building materials according to the present invention contains a large amount of salt, the shear bond strength, rate of change in length, rate of water retention, position correction degree and opening time required for the mortar composition, It can be seen that the quality standard of mortar (KS L 1592) is in conformity with or exceeded. Therefore, it can be concluded that it can be suitably used for bonding tiles or flooring materials.

이상과 같이, 본 발명은 비록 한정된 실시예에 의해 설명되었지만, 본 발명은 이것에 의해 한정되지 않으며, 본 발명이 속하는 기술분야에서 통상의 지식을 가진 자에 의하여 본 발명의 기술사상과 아래에 기재될 특허청구범위의 균등범위 내에서 다양한 수정 및 변형이 가능함은 물론이다.
Although the present invention has been described with reference to the exemplary embodiments, it is to be understood that the present invention is not limited thereto and that various changes and modifications may be made without departing from the spirit and scope of the present invention by those skilled in the art. And various modifications and variations are possible within the scope of the appended claims.



Claims (9)

소금 모르타르 조성물에 있어서,
녹말 12.5~15.0중량%, 설탕 6.5~11.5중량%, 다시마 추출물 12.5~17.5중량%, 찹쌀발아 7.5~12.5중량%, 솔잎 추출물 12.5~17.5중량%, 은행나무 추출물 2.5~5.0중량% 및 물 17.0~22.0중량%로 혼합되어 구성된 천연 혼합 추출물;
상기 천연 혼합 추출물 19.0~21.4중량%, 소금 70~75중량% 및 허브 오일 6~10중량%로 혼합하여 이루어지고,
상기 천연 혼합 추출물은 4일 내지 7일간 상온에서 숙성시켜 액상으로 형성되며, 상기 소금은 800℃ 내지 1,000℃에서 8시간 구운 천일염으로 이루어지는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
In the salt mortar composition,
A ginseng extract 12.5 to 17.5 wt.%, A glutinous rice germination 7.5 to 12.5 wt.%, A pine needle extract 12.5 to 17.5 wt.%, A ginkgo extract 2.5 to 5.0 wt.% And a water 17.0 to 15.0 wt. 22.0% by weight of a natural mixed extract;
19.0-21.4% by weight of the natural mixed extract, 70-75% by weight of salt and 6-10% by weight of herbal oil,
Wherein the natural mixed extract is aged at room temperature for 4 days to 7 days to be formed into a liquid phase, and the salt is made of a salt of sun dried salt at 800 ° C to 1,000 ° C for 8 hours.
제1 항에 있어서,
상기 허브 오일은 라벤더, 로즈마리, 민트, 구본초, 쑥, 솔잎으로 이루어진 군으로부터 선택되는 하나 이상의 혼합물로 이루어지는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
The method according to claim 1,
Wherein the herb oil is at least one compound selected from the group consisting of lavender, rosemary, mint, syrup, wormwood, pine leaf.
제1 항에 있어서,
상기 천연 혼합 추출물 및 이 천연 혼합 추출물과 소금 및 허브 오일의 혼합은 교반기에 의해서 30분 내지 60분 동안 300rpm 내지 900rpm의 교반 속도로 교반시켜 이루어지는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
The method according to claim 1,
Wherein the natural mixed extract and the natural mixed extract are mixed with salt and herbal oil by stirring at a stirring speed of 300 rpm to 900 rpm for 30 minutes to 60 minutes by a stirrer.
삭제delete 삭제delete 제1 항에 있어서,
상기 조성물은 전단 접착 강도가 0.40N/㎟ 내지 0.60N/㎟ 으로서, 파티션, 시멘트, 벽지 및 석고보드에 시공되는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
The method according to claim 1,
Wherein the composition has a shear bond strength of 0.40 N / mm < 2 > to 0.60 N / mm < 2 >, applied to partitions, cement, wallpaper and gypsum board.
제1 항에 있어서,
상기 조성물은 식용색소, 분말도료, 황토, 백토석 및 안료제의 군에서 선택되는 하나 이상의 추가의 성분을 포함하여 다양한 색상을 발현시키는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
The method according to claim 1,
The composition of claim 1, wherein the composition comprises at least one additional component selected from the group of food colors, powder coatings, loess, white pebbles and pigments.
제1 항에 있어서,
상기 천연 혼합 추출물은 증점제 성분을 추가로 혼합하여 접착력이 증대되는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.
The method according to claim 1,
Characterized in that the natural mixed extract is further mixed with a thickener component to increase the adhesive strength of the salt mortar composition.
제1 항에 있어서,
상기 소금 모르타르 조성물은 접착 시 서서히 굳어지면서 용해된 소금이 상온에서 재결정화되는 과정을 포함하여 이루어지는 것을 특징으로 하는 건축 자재용 소금 모르타르 조성물.





The method according to claim 1,
Wherein the salt mortar composition comprises a step of slowly solidifying the salt and recrystallizing the dissolved salt at room temperature.





KR1020150039838A 2015-03-23 2015-03-23 Salt mortar composition for building materials KR101529857B1 (en)