JPS63293113A - メタリック針布の焼入方法 - Google Patents

メタリック針布の焼入方法

Info

Publication number
JPS63293113A
JPS63293113A JP13048387A JP13048387A JPS63293113A JP S63293113 A JPS63293113 A JP S63293113A JP 13048387 A JP13048387 A JP 13048387A JP 13048387 A JP13048387 A JP 13048387A JP S63293113 A JPS63293113 A JP S63293113A
Authority
JP
Japan
Prior art keywords
tips
electrode
card clothing
torch
hardening
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP13048387A
Other languages
English (en)
Inventor
Yuzuru Nakano
中野 譲
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to JP13048387A priority Critical patent/JPS63293113A/ja
Publication of JPS63293113A publication Critical patent/JPS63293113A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は礒維産業の梳綿機に用いるメタリック針布の焼
入方法に関するものである。
〔従来の技術およびその問題点〕
従来、メタリック針布の歯先の硬度を高める焼入処理は
、都市ガスと酸素ガス等の混合ガスによる火焔を歯先の
部分に吹つけて加熱した後、急冷して焼入れしているが
、火焔の温度が低く加熱に時間が掛り、歯先部より歯底
部へ熱伝導が生じ、歯先部のみ焼入れすることが困難な
□るために、歯先よりの焼入部の寸法が浅かったり、又
歯先から縁部まで焼入されて使用不可能となるなど、焼
入の制御が極めて困難であった。
上記欠点を解消するために、レーザー光線を用いて歯先
部を焼入する方法が試みられているが、装置や運転費用
が極めて高価であり、使用方法も複雑で熟練を必要とし
、メタリック針布のような長尺物をg4時間連続焼入す
ることに種々の支障が生じ、実用化が困難である等の間
1点がある。
〔問題点を解決する為の手段〕
本発明は上記問題点を解決するため、空気。
酸素、窒素、水素等の気体をそれぞれ単独又は組合わせ
、これらの気体を電極とチップよりなるトーチより高速
、かつ細く絞ってメタリック針布の歯先部に吹き付けな
がらトーチ内の電極と歯先部間に通電し、プラズマアー
クを発生させ、歯先部を瞬間的に加熱後、急冷して焼入
することにより、歯先部のみ深く焼入し、縁部が焼入さ
nないメタリック針布の焼入方法を提供することによυ
問題点を解決したものである。
以下、本発明の一実施例を図面に従って説明する。
〔実施例〕
図面は本発明の実施の一例を示す概略斜視図である。図
面に示す様に、トーチ(1)内に設けた電極(2)と、
該電1@ fz)の下部を通過させるメタリック針布の
歯先部(3)を近接させて通過させるように配置し、電
極の周囲より空気(4)を高速、かつ細く絞って吹出さ
せ乍ら、電極と歯先部間に通電し、酸素プラズマアーク
(6)を発生させる。
メタリ、yり針布の歯先部(3)間のピッチは通常1〜
8絹と小さく、プラズマアーク1】が上記ピッチと同程
度であり、一旦通電してアークが発生すると、メタリッ
ク針布を移動させても、プラズマアークは連続して発生
し、歯先が連続的に加熱が行われる。歯先部が所定の寸
法迄、所定の焼入温度に達した後、冷水で急冷して焼入
を行う。
上記本発明の方法により、メタリック針布巾先部のみが
高硬変となった理想的なメタリック針布を得ることがで
きる。
また上記実施例においてプラズマアークは約2万度の高
温に達するのでトーチより吹出す気流を細く絞ることに
より、歯先部のみを瞬間に加熱することができる。
プラズマアークは空気以外に、酸素、窒素。
水素などの気体でプラズマ化するものが使用でき、加熱
時の歯先の酸化を少なくするときは窒素ガスなどの非酸
化性気体を使用するとよく、またこれらの気体を混合し
てもよい。またメタリック針布は適当な方法でアースし
ておく。
また本発明は焼入前後の焼鈍、焼戻などの熱処理にも適
用することができる。
〔発明の効果〕
本発明は上記の如くなしたから、従来のガス焔よりも極
めて細く、かつ高温状態に絞れるので、メタリック針布
の歯先部の所定寸法部分のみが加熱、焼入可能となシ、
縁部まで焼入されずに所定寸法を深く、かつ焼入時間が
短いので高硬度となり、メタリック針布の耐摩耗性を著
しく大きくできる。
さらに焼入れ装置は簡単で廉価であシ、堰扱いも容易な
るため、レーザー装置の如く、高価で複雑、危険な装置
を使用しないから運転、保守も容易でアシ、かつイニシ
ャルコスト、ランニングコストも少なくてすむ等の優れ
た効果を有する発明である。
【図面の簡単な説明】
図面は本発明の実施の1例を示す焼入工程の概略斜視図
である。

Claims (1)

    【特許請求の範囲】
  1. 空気、酸素、窒素、水素などの気体を、それぞれ単独に
    、またはこれらを組合せてなる混合気体を電極とチップ
    よりなるトーチより高速で且、細く絞って吹出させ、該
    トーチの下方に位置させて繰り出すメタリック針布と上
    記電極間に通電させることにより、これらの気体をプラ
    ズマアーク化し、メタリック針布の歯先を瞬間的に加熱
    した後、冷却媒体により急冷することを特徴とするメタ
    リック針布の焼入方法。
JP13048387A 1987-05-27 1987-05-27 メタリック針布の焼入方法 Pending JPS63293113A (ja)