JPS6242501A - Wound magnetic core for control - Google Patents

Wound magnetic core for control

Info

Publication number
JPS6242501A
JPS6242501A JP60182330A JP18233085A JPS6242501A JP S6242501 A JPS6242501 A JP S6242501A JP 60182330 A JP60182330 A JP 60182330A JP 18233085 A JP18233085 A JP 18233085A JP S6242501 A JPS6242501 A JP S6242501A
Authority
JP
Japan
Prior art keywords
magnetic core
magnetic field
control
iron loss
amorphous metal
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP60182330A
Other languages
Japanese (ja)
Other versions
JPH0669004B2 (en
Inventor
Katsuto Yoshizawa
克仁 吉沢
Susumu Nakajima
晋 中島
Kiyotaka Yamauchi
山内 清隆
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Proterial Ltd
Original Assignee
Hitachi Metals Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Metals Ltd filed Critical Hitachi Metals Ltd
Priority to JP60182330A priority Critical patent/JPH0669004B2/en
Publication of JPS6242501A publication Critical patent/JPS6242501A/en
Priority to US07/085,405 priority patent/US4769091A/en
Publication of JPH0669004B2 publication Critical patent/JPH0669004B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To decrease the iron-loss and increase the rectangular ratio by a method wherein a thin piece of amorphous metal with a specified composition formula is cooled passing through Curie temperature while applying a magnetic field, and then it is held in the magnetic field. CONSTITUTION:In the amorphous metal whose composition is expressed in the formula, x, y, and z each indicate atom %. A thin metal piece with relation, 0<=a<=0.05, 0.03<=b<=0.08 and 13<=x<=16, 7.5<=y<=9.5, 1.0<=z<=3 is held in over Curie temperature. After that, it is gradually cooled while alteration or direct magnetic field with specified strength is applied in the direction of the magnetic path. After being held within a specified temperature range for a period of time, the piece is cooled to a room temperature to form a winding magnetic core for control. With this method, iron-loss is reduced to form a winding magnetic core with large rectangular ratio.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は、磁気制御型スイッチング電源等に組み込まれ
る可飽和リアクトル等に使用される制御用巻磁心の改良
に関するものであシ、特に、経時変化が小さく、鉄損が
特に小さい高角形比制御用巻磁心を提供するものである
。
[Detailed Description of the Invention] [Field of Industrial Application] The present invention relates to the improvement of a control wound core used in a saturable reactor incorporated in a magnetically controlled switching power supply, etc. The object of the present invention is to provide a wound core for high squareness ratio control that has small changes and particularly low iron loss.

〔従来の技術〕[Conventional technology]

従来、制御用磁心としては50%Ni系A?−マロイ、
80%Ni系ノJ?−マロイの巻磁心が主に使用されて
いたがこれらは50kHz以上の高周波交番磁場で駆動
した場合には鉄損が著しく大きくなるために、最近では
高周波特性に秀れるアモルファス金属製巻磁心が使用さ
れはじめている。
Conventionally, the control magnetic core was made of 50% Ni-based A? - Malloy,
80% Ni type J? - Malloy wound cores were mainly used, but when these are driven with a high frequency alternating magnetic field of 50kHz or higher, iron loss becomes significantly large, so recently amorphous metal wound cores, which have excellent high frequency characteristics, are being used. It's starting to happen.

〔発明が解決しようとする問題点〕[Problem that the invention seeks to solve]

制御用磁心に適したアモルファス金属磁心を製造するた
めの熱処理方法としては、特公昭59−29644号(
増水、藤森)に示されているような磁場中熱処理方法が
知られている。ここには、磁場中で一定温度区間を一定
の冷却温度で冷却する方法が開示されている。この方法
によれば、高角形比で直流B−Hカーブの保磁力の小さ
いアモルファス金属材料が得られる。
As a heat treatment method for producing an amorphous metal magnetic core suitable for a control magnetic core, Japanese Patent Publication No. 59-29644 (
A method of heat treatment in a magnetic field is known, such as the one shown in Kosui, Fujimori). This document discloses a method of cooling a constant temperature section at a constant cooling temperature in a magnetic field. According to this method, an amorphous metal material having a high squareness ratio and a small coercive force in the DC B-H curve can be obtained.

本発明は、直流B−Hカーブの保磁力よりもむしろ、交
流B−He性の保磁力(He)に着目して、50 kH
z以上の高周波で駆動した場合に特に鉄損が少なく、高
角形比(Br/Bs)を有する制御用磁心を提供するも
のである。(ここで、Brは残留磁束密度、Baは飽和
磁束密度を表わす。)本発明は、50 kHz以上の高
周波で駆動するスイッチング電源用可飽和リアクトルに
使用した場合、温度上昇が少なく、利得が十分ある制御
用巻磁心を提供する。
The present invention focuses on the coercive force (He) of the AC B-He property rather than the coercive force of the DC B-H curve.
The present invention provides a control magnetic core that has particularly low iron loss and a high squareness ratio (Br/Bs) when driven at a high frequency of z or higher. (Here, Br represents the residual magnetic flux density, and Ba represents the saturation magnetic flux density.) When the present invention is used in a saturable reactor for a switching power supply driven at a high frequency of 50 kHz or higher, the temperature rise is small and the gain is sufficient. A control wound core is provided.

〔問題点を解決するための手段〕[Means for solving problems]

本発明においては、合金組成として(X * 7 +2
は各々原子チを示す)、 組成式: (col−a−br・aMtl B )10
0−x−y−s S l x B yMOz但し、O≦
龜≦0.05 、0.03≦b≦O,OS。
In the present invention, the alloy composition is (X * 7 + 2
each represents an atom), compositional formula: (col-a-br・aMtl B )10
0-x-y-s S l x B yMOzHowever, O≦
龜≦0.05, 0.03≦b≦O, OS.

13≦X≦16.7.5≦y≦9.5 、1.0≦2≦
3を有するものが合金として適当である。Fa基アモル
ファス合金とは相異してCo基アモルファス合金におい
ては、保磁力(He )が小さく、角形比(Br/’B
s )の大きいものが得られやすい。Co基アモルファ
ス合金においては、coの1部をFe及びMnで置換す
ることによシ、磁歪(λ11)が小さい磁心材料とする
ことが出来る。81は、合金の鉄損を低減するのに効果
があるが、過多に含有されると合金のキュリ一温度(T
c)を下げ、角形比(Br/US)を著しく低下させる
。以上の様なことから、S1含有量は合金に望ましい特
性を付与するためには、13〜16原子チが好ましい。
13≦X≦16.7.5≦y≦9.5, 1.0≦2≦
3 is suitable as an alloy. Unlike Fa-based amorphous alloys, Co-based amorphous alloys have a small coercive force (He) and a squareness ratio (Br/'B
s) is likely to be obtained. In a Co-based amorphous alloy, by substituting a part of Co with Fe and Mn, a magnetic core material with small magnetostriction (λ11) can be obtained. 81 is effective in reducing the iron loss of the alloy, but if it is contained in an excessive amount, the Curie temperature (T
c) and significantly reduce the squareness ratio (Br/US). From the above, the S1 content is preferably 13 to 16 atoms in order to impart desirable properties to the alloy.

B含有量については7.5原子チよシ少ないと合金をア
モルファス状態にすることがむずかしく、又、逆に、9
.5原子チよυ多いと磁束密度(Ba)の低下をもたら
すので、7.5〜9.5原子チとする。
Regarding the B content, if it is less than 7.5 atoms, it is difficult to make the alloy into an amorphous state;
.. If there are more than 5 atoms, the magnetic flux density (Ba) will decrease, so it is set to 7.5 to 9.5 atoms.

Coの1部をF@で置換することによシ、飽和磁束密度
(B8)を増大させることが出来るがFa量aが0.0
5を越えると経時変化が大きくなるためaは0.05以
下が望ましい。又、coの1部をMnで置換することに
より、F・との関係で、磁束(λS)を著しく小さくす
ることが出来るが、Mn Ilbが0.03未満では鉄
損の増加をまねき、O,OSを越えるとアモルファスリ
ゲンが脆化しやすくなる。
By replacing a part of Co with F@, the saturation magnetic flux density (B8) can be increased, but when the amount of Fa is 0.0
If it exceeds 5, the change over time becomes large, so it is desirable that a is 0.05 or less. Furthermore, by substituting a part of co with Mn, the magnetic flux (λS) can be significantly reduced in relation to F. However, if Mn Ilb is less than 0.03, iron loss increases and O , OS is exceeded, amorphous regen becomes easily brittle.

F・置換量は、Coに対して5チまでが望ましく、Mn
置換量は、Coに対して、3チ以上、8%以下が適当で
ある。
The amount of F substitution is preferably up to 5% for Co, and Mn
The appropriate amount of substitution with respect to Co is 3% or more and 8% or less.

Mo添加は、交流B−Hカーブにおける保磁力(He)
を減少させるのに極めて効果が有る。1.0原子チ以上
のMo添加によシ保磁力(He )を無添加の場合に比
較して70%も減少させることが出来得る。この保磁力
(Hc)の減少効果に伴なって、鉄損が大幅に減少する
。過多に添加した場合には残留磁束密度(Br)及び角
形比(Br/Bs )の低下が著しくなるので、3原子
チ以下とする。
Mo addition increases the coercive force (He) in the AC B-H curve.
It is extremely effective in reducing By adding 1.0 or more atoms of Mo, the coercive force (He) can be reduced by as much as 70% compared to the case without addition. Along with this effect of reducing coercive force (Hc), iron loss is significantly reduced. If too much is added, the residual magnetic flux density (Br) and the squareness ratio (Br/Bs) will be significantly lowered, so the content should be 3 atoms or less.

Mo添加は、Nb又はSk添加に比較して、交流B−H
カーブの保磁力(Ha)を減少させる効果は大きく、一
方、角形比(Br/Bs )の減少は小さいので、特に
有利である。
Compared to Nb or Sk addition, Mo addition reduces AC B-H
This is particularly advantageous since the effect of reducing the coercive force (Ha) of the curve is large, while the reduction in squareness ratio (Br/Bs) is small.

本発明合金の熱処理としては鋳造後キュリ一温度(Tc
)以上で保持後磁場中徐冷した後、磁場中で0.95 
X Tc ℃〜150℃の範囲内で1時間〜10時間保
持した後室温まで冷却する。
The heat treatment for the alloy of the present invention includes Curie temperature (Tc) after casting.
) After holding in a magnetic field and cooling slowly in a magnetic field, the temperature was 0.95
X Tc The temperature is maintained within the range of 150°C to 150°C for 1 hour to 10 hours, and then cooled to room temperature.

磁場をかけながらキュリ一温度(Ta)を通過して冷却
し、その後、磁場中で保持することにより、鉄損を減少
させ、角形比(Br/Bs )を高めることが出来る。
By cooling the material through the Curie temperature (Ta) while applying a magnetic field and then holding it in the magnetic field, iron loss can be reduced and the squareness ratio (Br/Bs) can be increased.

〔実施例〕〔Example〕

以下、本発明を実施例に従って説明する。 Hereinafter, the present invention will be explained according to examples.

実施例1 単ロール法によシ組成式: %式% わされるアモルファス金属リボンを作成し、磁路長方向
に磁場をかけながら、キュリ一温度(Tc )以上で熱
処理した後に約Q、8XTc℃で1.5時間磁場中保持
した後、室温まで冷却した。
Example 1 An amorphous metal ribbon was prepared using a single roll method, and was heat-treated at a temperature higher than the Curie temperature (Tc) while applying a magnetic field in the direction of the magnetic path length. After being held in a magnetic field for 1.5 hours at °C, it was cooled to room temperature.

第1図に角形比(Br/13++ ) 、鉄損(W)、
及び交流B−Hカーブにおける保磁力(He)に対する
添加元素Mの種類及び含有量Xに対する依存性を示す。
Figure 1 shows the squareness ratio (Br/13++), iron loss (W),
and the dependence of the coercive force (He) on the type and content X of the additive element M in the AC B-H curve.

Crは鉄損(W)及び保磁力(Hc)を低下させるのに
効果があるが、角形比(B r/B s )を大幅に低
下させてしまうので、望ましくない。Nbは、Crに比
較して角形比(Br/Bs )の低下はやや少ないが、
Moに比較するとやや大ぎい。Moは、交流B−Hカー
ブにおける保磁力(He)を減少せしめ、鉄損(W)を
減少せしめる一方、角形比(Br/Bs )の低下は他
の添加元素Cr、Nbに比較して少ないので好適な添加
元素である。
Although Cr is effective in reducing iron loss (W) and coercive force (Hc), it is undesirable because it significantly reduces the squareness ratio (B r /B s ). Nb has a slightly lower squareness ratio (Br/Bs) than Cr, but
It is slightly larger than Mo. Mo decreases the coercive force (He) in the AC B-H curve and decreases the iron loss (W), while the decrease in the squareness ratio (Br/Bs) is smaller than that of other additive elements Cr and Nb. Therefore, it is a suitable additive element.

実施例2 実施例1におけると同様にして、組成式:%式% 明アモルファス合金を作成し、50 % Nl系74′
−マロイ、80%Ni系・ぐ−マロイとの特性比較を行
なった結果を第1表に示す。
Example 2 In the same manner as in Example 1, a bright amorphous alloy with a compositional formula: % formula % was prepared, and 50% Nl-based 74'
Table 1 shows the results of a comparison of the characteristics of -Malloy and 80% Ni-based G-Malloy.

又、比較材として、組成式: ”70”0.4”6S113B8.75NbL85のア
モルファス合金を作成し、その特性も第1表に示す。
In addition, as a comparison material, an amorphous alloy having the composition formula: "70"0.4"6S113B8.75NbL85 was prepared, and its properties are also shown in Table 1.

第1表から明らかな様にパーマロイ系材料は、20 k
Hz程度の低い周波数の交番磁場しか使用出来ないか、
或いは、角形比が60チ程度と低い値であるので高周波
スイッチング駆動には適さない。
As is clear from Table 1, the permalloy material is 20k
Can only an alternating magnetic field with a low frequency of about Hz be used?
Alternatively, since the squareness ratio is as low as about 60 inches, it is not suitable for high frequency switching drive.

一方、本発明材は、角形比93%と云う様に比較用アモ
ルファス合金材又は、50%N i 系/#−マロイ並
みであり、一方、鉄損は比較用アモルファス合金材に比
較して、25%と云う様に著しく小さくなっている。経
時変化もほとんどなく、比較用アモルファス合金材、5
0%Ni系・ぞ−マロイ並みであり100〜200 k
Hz位が適正駆動周波数である。
On the other hand, the present invention material has a squareness ratio of 93%, which is comparable to the comparison amorphous alloy material or 50% Ni system/#-malloy, and on the other hand, the iron loss is as compared to the comparison amorphous alloy material. It is significantly smaller at 25%. Comparative amorphous alloy material with almost no change over time, 5
0%Ni type, similar to Malloy, 100-200k
Approximately Hz is the appropriate driving frequency.

実施例3 実施例1におけると同様にして、 本発明材’ (”0.925Fe0.025Mn0.0
5)73.5MO2,5S115B9の板厚を種々変化
させて、交流B−Hカーブの保磁力(He)、及び鉄損
(W)の板厚依存性測定した。
Example 3 In the same manner as in Example 1, the present invention material'("0.925Fe0.025Mn0.0
5) The plate thickness of 73.5MO2, 5S115B9 was varied and the dependence of the coercive force (He) and iron loss (W) of the AC B-H curve on the plate thickness was measured.

結果を第2図に示す。同図には比較の為、組成式=Co
70”0.4”4”l!SB8.75NbIJ15なる
合金組成のアモルファス合金の板厚依存性を示す。本発
明材においては、特に、す?ン板厚が25μm以下のも
のにおいて、特に交流B−Hカーブの保磁力(He)の
小さいものが得られる。板厚5μmよシ小さいものは、
単ロール法による作成はむずかしい。
The results are shown in Figure 2. For comparison, the figure shows the composition formula = Co
70"0.4"4"l!SB8.75NbIJ15 The plate thickness dependence of an amorphous alloy with an alloy composition of -H curve with small coercive force (He) can be obtained.Thickness as small as 5 μm can be obtained by
It is difficult to make using the single roll method.

実施例4 実施例1におけると同様にして、本発明材と比較用アモ
ルファス合金材及び50チNi系パーマロイ、80ts
NI系パーマロイを作成し、印加する交流磁場の周波数
に対して、これら材料の鉄損(W)がどのように変化す
るかを測定した。その結果を第3図に示す。第3図に示
されるように横軸を交流磁場の周波数として縦軸に鉄損
(W)をログ・スケールで取った場合に、鉄損は周波数
増加に対応して、はぼ直線的に増加するが、本発明材は
高周波交流磁場に対してもコア、ロスが他材料に比較し
て小さいので、100 kHz又は200 kHz等高
周波で駆動するに特に好適である。
Example 4 In the same manner as in Example 1, the present invention material, a comparative amorphous alloy material, 50ts Ni-based permalloy, and 80ts
We created NI-based permalloy and measured how the iron loss (W) of these materials changes with the frequency of the applied alternating current magnetic field. The results are shown in FIG. As shown in Figure 3, when the horizontal axis is the frequency of the alternating magnetic field and the vertical axis is the iron loss (W) on a log scale, the iron loss increases almost linearly as the frequency increases. However, since the material of the present invention has a smaller core loss than other materials even in the case of high-frequency alternating magnetic fields, it is particularly suitable for driving at high frequencies such as 100 kHz or 200 kHz.

本発明材では、100 kHzの交番磁場を印加した場
合の鉄損(W)が500kW/rn3以下のものが容易
に得られる。第4図に本発明の熱処理パターンの一例を
示す。
With the material of the present invention, one with an iron loss (W) of 500 kW/rn3 or less when a 100 kHz alternating magnetic field is applied can be easily obtained. FIG. 4 shows an example of the heat treatment pattern of the present invention.

〔発明の効果〕〔Effect of the invention〕

以上、本発明を実施例に基づいて説明したが、本発明材
は従来材料に比較して経時変化、角形比は同等であるが
交流B−Hカーブの保磁力(He)及び鉄損(W)は著
しく小さいものであり、特に高周波駆動用磁気増幅方式
スイッチング電源用制御用磁心として最適である。
The present invention has been explained above based on examples, but the present invention material has the same change over time and squareness ratio as the conventional material, but the coercive force (He) and iron loss (W) of the AC B-H curve. ) is extremely small, making it particularly suitable as a control core for magnetic amplification type switching power supplies for high-frequency drives.

図面の簡単な説明 第1図は組成式: %式% Nb又はMo)を有するアモルファス合金の角形比(B
r/Ba ) 、鉄損(W)、及び交流B −Hカーブ
の保磁力(He)を示す図、第2図は、本発明材及び比
較材の保磁力(Hc)、鉄損(W)の板厚依存性を示す
図、第3図は本発明合金材、比較材、50%Nl系ノや
−マロイ材、80チNi系ノ譬−マロイ材のシ、;−4
;イ ー−=/ 第 1 目 (Coo、q2  Feo、、5 △グn o、 o 
ys)76−xハイx 5Lyczs  B、ysX(
al  %) 第3図 f(kHz)
Brief explanation of the drawings Figure 1 shows the squareness ratio (B
Figure 2 shows the coercive force (Hc), iron loss (W) of the present invention material and comparative material. Figure 3 is a diagram showing the dependence of plate thickness on the alloy material of the present invention, comparative material, 50% Nl-based malloy material, 80% Ni-based malloy material; -4
;E-=/ 1st (Coo, q2 Feo, 5 △gun o, o
ys) 76-x high x 5Lyczs B, ysX(
al %) Figure 3 f (kHz)

Claims (1)

【特許請求の範囲】 1、組成式: (Co_1_−_a_−_bFe_aMn_b)_1_
0_0_−_x_−_y_−_zSi_xB_yMo_
z但し、0≦a≦0.05、0.03≦b≦0.08、
13≦x≦16、7.5≦y≦9.5、1.0≦z≦3
の関係を有するアモルファス金属薄帯片を巻いたもので
、キュリー温度以上で保持後、磁路方向に0.10e以
上の交流あるいは直流の磁界を印加しながら冷却速度0
.1℃/分〜50℃/分で徐冷後、0.95×Tc℃〜
150℃の範囲内で1時間〜10時間保持した後、室温
まで冷却して形成したことを特徴とする制御用磁心。 2、アモルファス金属薄帯片の板厚が5μm〜25μm
であることを特徴とする特許請求の範囲第1項記載の制
御用巻磁心。 3、周波数100kHz、磁束密度の波高値Bmが2k
Gの場合の鉄損(W)が500kW/m^3以下である
ことを特徴とする特許請求の範囲第1項記載の制御用巻
磁心。
[Claims] 1. Composition formula: (Co_1_-_a_-_bFe_aMn_b)_1_
0_0_-_x_-_y_-_zSi_xB_yMo_
zHowever, 0≦a≦0.05, 0.03≦b≦0.08,
13≦x≦16, 7.5≦y≦9.5, 1.0≦z≦3
It is a wound amorphous metal thin strip having the relationship of
.. After slow cooling at 1°C/min to 50°C/min, 0.95×Tc°C to
A control magnetic core characterized in that it is formed by maintaining the temperature within a range of 150°C for 1 to 10 hours and then cooling it to room temperature. 2. The thickness of the amorphous metal thin strip is 5 μm to 25 μm.
A control wound magnetic core according to claim 1, characterized in that: 3. Frequency: 100kHz, peak value Bm of magnetic flux density: 2k
The control wound magnetic core according to claim 1, characterized in that the iron loss (W) in the case of G is 500 kW/m^3 or less.
JP60182330A 1985-08-20 1985-08-20 Manufacturing method of control winding core Expired - Lifetime JPH0669004B2 (en)