JPH11185738A - 鉛蓄電池 - Google Patents
鉛蓄電池Info
- Publication number
- JPH11185738A JPH11185738A JP9354417A JP35441797A JPH11185738A JP H11185738 A JPH11185738 A JP H11185738A JP 9354417 A JP9354417 A JP 9354417A JP 35441797 A JP35441797 A JP 35441797A JP H11185738 A JPH11185738 A JP H11185738A
- Authority
- JP
- Japan
- Prior art keywords
- negative electrode
- lead
- charge
- battery
- active material
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
足傾向となり、電池の短寿命化に至るという問題を解消
することを課題とする。 【解決手段】 負極活物質に添加されているリグニン化
合物は電池を充電する際の充電受け入れ性を低下させる
が、リグニン化合物の負極活物質に添加する量を0.0
1%〜0.07%とすることにより、充電受け入れ性を
向上させて充電不足になり難い電池を得る。
Description
のである。
放電状態(PbSO4 )から充電状態(Pb)に変化す
る際に負極活物質の収縮現象が発生して比表面積が減少
する。また自動車の電池の使用用途としては主としてエ
ンジン始動時の高率放電があり、活物質の内部と表面部
とで、この活物質の収縮度合が異なってくる。このた
め、充電放電の繰り返しの中で負極活物質自体の導電性
の低下を促し、放電特性の低下,寿命特性の短寿命化に
至るという問題があった。そこで、負極活物質の防縮剤
としてリグニンスルホン酸塩を主原料としたリグニン化
合物を添加して、負極活物質の比表面積低下を抑制し
て、それまでの鉛蓄電池の放電特性,寿命を向上させて
きた。
池には近年ではエンジン始動を頻繁に行うような特殊な
用途も生じてきた。これは電池に対して深い放電を幾度
も繰り返すような使用方法であり、このような使用では
充電不足傾向となり早期での寿命劣化に至る原因ともな
っている。そこで充電不足傾向を解消するために充電時
の充電受け入れ性を向上することが課題となっており、
鉛蓄電池の負極活物質の防縮剤としてリグニン化合物を
添加しているが、リグニン化合物がPb2+ に吸着し
て、充電時の充電受け入れ性を低下させるという問題が
あった。
決するために負極活物質に添加するリグニン化合物の最
適量を見出したものである。これにより、充電時の充電
受け入れ性が向上して、結果として深い放電を繰り返さ
れたとしても、走行時等に高率良く充電することができ
て、充電不足になり難い電池を得ることができる。
質の添加剤であるリグニン化合物の量を従来よりも少な
い0.01%〜0.07%とすることにより、電池とし
ての充電受け入れ性を向上させたものである。
例について以下に説明する。
(社)製のリグニン化合物(商品名バニレックス)の他
に常法に従ってカーボン,硫酸バリウム,ポリエステル
短繊維を鉛および鉛酸化物の混合粉体中に撹拌混合して
硫酸と水で練合して負極活物質ペーストを得た。リグニ
ン化合物の添加量を表1に示す。
に対するリグニン化合物の量を重量百分率で示してい
る。すなわち、本発明の実施例1では0.01%、本発
明の実施例2では0.03%、本発明の実施例3では
0.05%、本発明の実施例4では0.07%、比較例
では0.09%、従来例では0.10%とする。
−Ca−Sn系合金格子に塗着することにより作製した
負極板と正極板およびセパレータを重ね合わせてJIS
規格(D 5301)にて定められた55D23の各電
池を得た。次に上記の各電池を40℃雰囲気中で19.
2A(終止電圧7.2V)で1時間の放電と、14.8
V(最大電流24A)で2時間の充電を繰り返す充放電
を行って深放電型のサイクル寿命特性を各電池について
調べた。表1および図1にそれらの結果を示す。表1お
よび図1の結果から負極活物質中のリグニン含有率が
0.01%〜0.07%の本発明の実施例による電池に
ついてサイクル寿命特性の大幅な向上が見られた。また
0.01%〜0.05%の本発明の実施例による電池の
場合は、さらにサイクル数が延びる結果が得られた。こ
れは充電受け入れ性の向上により充電がされ易くなり、
従来例のように問題となってきた充電不足が解消された
ことによる。実際、寿命試験初期における充電電気量を
調査したところ、従来例のリグニン含有率が0.10%
の電池であると充電電気量百分率(充電電気量/放電電
気量×100)にして103%、それに対してリグニン
含有量を減少させるに従って、表2のように充電電気量
百分率は増加して106.5%にまで増加することがわ
かる。
電気量百分率は3%前後の差であるが、これが寿命サイ
クル数の進行の中で充電過不足状態に大きく左右して寿
命特性に影響していると考えられる。
0%以上となるような深い放電と定電圧充電を繰り返す
ような深放電型の使用形態において負極添加物による負
極の充電受け入れ性を制御することにより、寿命が著し
く改善できるという知見は今までに得られていない。特
にアンチモンタイプの電池といった負極格子体にPb−
Sb系合金を用いる電池では、負極板の水素過電圧の低
下により電池の充電電圧が低下し、見かけより充電受け
入れ性が向上するために本発明に記載するような形での
寿命への影響はさほど大きくないが、負極格子体にアン
チモンを含まないPb−Ca−Sn系合金を用いるハイ
ブリッドタイプおよびカルシウムタイプの電池に本発明
の効果が有効である。とりわけ近年普及が著しい正,負
極格子体ともにアンチモンを含まないPb−Ca−Sn
系合金を用いたカルシウムタイプの電池では充放電時に
おける正極格子からのアンチモンの溶出,負極での析出
という機構がはたらかないため、本発明の効果は極めて
重要なものとなる。
れ性を向上させたことにより、充電不足となり難い鉛蓄
電池を提供することが可能となる。
寿命特性の関係を示す図
Claims (3)
- 【請求項1】 鉛蓄電池の負極活物質原料としての鉛お
よび鉛酸化物の混合粉体中に重量百分率で0.01%〜
0.07%のリグニン化合物を添加したことを特徴とし
た鉛蓄電池。 - 【請求項2】 鉛蓄電池の負極活物質原料としての鉛お
よび鉛酸化物の混合粉体中に重量百分率で0.01%〜
0.05%のリグニン化合物を添加したことを特徴とし
た請求項1記載の鉛蓄電池。 - 【請求項3】 負極格子体がPb−Ca−Sn系合金で
ある請求項1または2記載の鉛蓄電池。