JP4250057B2 - Household hygiene tissue paper - Google Patents
Household hygiene tissue paper Download PDFInfo
- Publication number
- JP4250057B2 JP4250057B2 JP2003364469A JP2003364469A JP4250057B2 JP 4250057 B2 JP4250057 B2 JP 4250057B2 JP 2003364469 A JP2003364469 A JP 2003364469A JP 2003364469 A JP2003364469 A JP 2003364469A JP 4250057 B2 JP4250057 B2 JP 4250057B2
- Authority
- JP
- Japan
- Prior art keywords
- paper
- strength
- paper strength
- wet
- pulp
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
本発明は、ロールペーパー、ティッシュペーパー、ちり紙等の家庭用衛生薄葉紙に係り、詳しくは高米坪でありながら、柔軟で手触り感が良好で、かつ吸水性に優れるとともに、強度特性に優れた衛生薄葉紙に関する。 The present invention relates to household hygiene thin paper such as roll paper, tissue paper, and dust paper. More specifically, it is a high hygiene, yet it is flexible, has a good touch feeling, has excellent water absorption, and has excellent strength characteristics. Related to tissue paper.
従来より、家庭用衛生薄葉紙として、ティッシュペーパー等が市場に多く提供されている。この種の衛生薄葉紙の場合には特に、柔らかさ、手触り感が良好であると同時に、吸水性が良好であり、使用時に破れが生じない程度の紙強度が要求される。 Conventionally, many tissue papers have been provided on the market as household sanitary thin paper. Particularly in the case of this type of sanitary thin paper, softness and touch feeling are good, and at the same time, water absorption is good, and paper strength is required such that tearing does not occur during use.
一般的に柔らかさ、手触り感を向上させるには、パルプスラリーに脂肪酸エステル系柔軟剤、ポリリン酸塩、ポリシロキサン、第4級アンモニウム塩型カチオン性界面活性剤などの紙用柔軟剤を添加する方法が採用され、シート強度を向上させるには、ポリアクリルアマイド、ポリアミン、エピクロロヒドリン樹脂等の紙力増強剤を添加する方法が採用されているが、前記柔らかさ、手触り感などの感触性能と、強度性能とは相反する特性であり、両者をバランス良く両立させることは難しいのが現状である。 In general, in order to improve softness and feel, paper softeners such as fatty acid ester softeners, polyphosphates, polysiloxanes, and quaternary ammonium salt type cationic surfactants are added to the pulp slurry. In order to improve the sheet strength, a method of adding a paper strength enhancer such as polyacrylamide, polyamine, epichlorohydrin resin, etc. is adopted. Performance and strength performance are contradictory properties, and it is difficult to achieve a good balance between the two.
この課題を解決するために、例えば下記特許文献1では、パルプ成分の60重量%以上が広葉樹化学パルプからなるパルプスラリーに、対パルプ当り0.05〜0.5重量%のカチオン化変成澱粉を配合して抄紙し、次いでソフトカレンダー処理することで柔軟性、手触り感およびシート強度に優れたティッシュペーパーを得る製造方法が提案されている。また、下記特許文献2では、ヤンキー抄紙機によりリグノセルローズ繊維を原料としてティシュウエブを抄紙し、次いでヤンキー抄紙機でのオンマシンカレンダー処理及び/又はプライマシンによるカレンダー処理によってトータルで2スタック以上のソフトカレンダー処置を行い、次いで折り板方式加工機で加工することにより、製品紙箱容積基準の嵩密度が0.12g/cm3以上である圧縮ティッシュペーパー束を形成し、箱詰めした2枚重ねの圧縮ティッシュペーパー製品の製造方法が提案されているが十分な効果は得られていない。 In order to solve this problem, for example, in Patent Document 1 below, 0.05 to 0.5% by weight of cationized modified starch per pulp is added to a pulp slurry in which 60% by weight or more of pulp components are made of hardwood chemical pulp. There has been proposed a production method for obtaining a tissue paper excellent in flexibility, touch feeling and sheet strength by blending and making paper, and then soft calendering. Further, in Patent Document 2 below, a tissue web is made from lignocellulosic fiber as a raw material by a Yankee paper machine, and then a total of two or more stacks by on-machine calendar processing and / or calendar processing by a ply machine. By performing calendar treatment and then processing with a folding plate type processing machine, a compressed tissue paper bundle having a bulk density of 0.12 g / cm 3 or more based on the volume of the product paper box is formed and packed in two stacked compressed tissues Although a method for producing a paper product has been proposed, a sufficient effect has not been obtained.
さらに、一般家庭において、ティッシュペーパーの使用用途を改めてアンケート調査してみると、例えば風邪などの際に鼻をかんだりしたり、化粧落しなどに使用されていることはもちろんであるが、かなりの割合で、テーブルや床などにこぼした液体の拭き取りに使用されている実態が浮き彫りとなった。
上記使用用途のアンケート調査に鑑み、一般家庭におけるティッシュペーパーの強度を使用実態に沿うように上げる必要がある。さらに、ワイプとしての機能をも持たせるようにするには、ティッシュペーパーの強度を上げるとともに、液体の吸水性を向上させる必要性が生じる。これを解決する手段として米坪を上げる方法が考えられるが、単に米坪を上げるとシートは硬くなってしまい、鼻をかんだり、化粧落しなどの際に非常に使用感に支障がでるようになる。したがって、米坪を上げても、ティッシュペーパーとして十分な柔軟性と肌触り感を満足するものでなくてはならない。 In view of the above-mentioned questionnaire survey of usage, it is necessary to increase the strength of tissue paper in general households to match the actual usage. Furthermore, in order to provide a function as a wipe, it is necessary to increase the strength of the tissue paper and improve the water absorption of the liquid. As a means to solve this, a method of raising the rice tsubo can be considered, but simply raising the rice tsubo will make the sheet harder, so that it will hinder the feeling of use when biting the nose or removing makeup, etc. Become. Therefore, even if the tsubo is raised, the tissue paper must satisfy sufficient flexibility and feel.
シートの柔軟性や手触り感を向上させる手段としては、前記特許文献1や特許文献2に記載された方法が存在する。しかし、これらの製造方法は、1枚当たりの米坪が11〜16g/m2の一般的なティッシュペーパーに対するものであり、1枚当たりの米坪が例えば15〜50g/m2としたティッシュペーパーに適用した場合には、紙の表面において繊維同士の水素結合が弱まる傾向を示すため、ワイプとして十分な表面強度特性を得ることができないという問題があった。 As means for improving the flexibility and feel of the sheet, there are methods described in Patent Document 1 and Patent Document 2. However, these methods of preparation, basis weight per sheet is intended for common tissue paper of 11~16g / m 2, tissue paper basis weight per sheet, for example, which was 15 to 50 g / m 2 When applied to No. 1, the hydrogen bond between fibers tends to be weakened on the surface of the paper, so that there is a problem that sufficient surface strength characteristics cannot be obtained as a wipe.
そこで、本発明の主たる課題は、米坪量が高い場合であっても、柔軟で手触り感が良好でありながら、強度特性(湿潤強度、乾燥強度及び表面特性等)が良好で、かつ吸水性に優れた家庭用衛生薄葉紙を提供することにある。 Therefore, the main problem of the present invention is that even when the basis weight of rice is high, the strength characteristics (wet strength, dry strength, surface characteristics, etc.) are good and water absorption is good while being soft and having a good touch feeling. It is to provide an excellent household sanitary thin paper.
前記課題を解決するために請求項1に係る本発明として、1枚当たりの米坪が15〜50g/m2であり、乾燥紙力(縦方向)が400〜1400cN、乾燥紙力(横方向)が200〜500cN、湿潤紙力(縦方向)が150〜500cN、湿潤紙力(横方向)が50〜300cNであり、かつ吸水度が0.1〜1.5秒である紙質を備える家庭用衛生薄葉紙であって、
フリーネスが630cc以上としたパルプ主原料に、湿潤紙力増強剤としてポリアミドポリアミンエピクロルヒドリン樹脂を2.0〜20.0kg/t、カチオン系柔軟剤を0.1〜20.0kg/t添加するとともに、エーテル化度0.3〜0.9のCMC(カルボキシメチルセルロース)又はその塩を0.1〜20.0kg/t添加し、
カレンダー処理条件におけるカレンダー種別がソフトカレンダー又は金属カレンダーとし、ニップ線圧が7〜30kgf/cm、ニップ数が1〜3、マシンスピードが300〜2000m/分として抄紙したことを特徴とする家庭用衛生薄葉紙が提供される。ここで、前記吸水度は次記(1)〜(5)の工程を経て得た値である。
(1)測定器具としてデジタルマイクロピペット、ストップウォッチ、三脚台を使用する。
(2)試料2枚重ねを一組として中央部直径40mm以上の穴のある支持台に置く。
(3)デジタルマイクロピペットに蒸留水を取り、約10mmの高さから試験片に蒸留水を1滴(0.1ml)滴下する。
(4)水滴が試験片に接触した瞬間から、水が完全に吸収されて紙表面の反射が消えるまでの時間をストップウォッチで0.01秒単位で測定する。
(5)試験は5回行い、その平均値を小数点第1位まで記録する試験要領によって得た数値とする。
In order to solve the above-mentioned problems, the present invention according to claim 1 has a rice basis weight of 15-50 g / m 2 per sheet, a dry paper strength (longitudinal direction) of 400-1400 cN, and a dry paper strength (lateral direction). ) Is 200 to 500 cN, wet paper strength (longitudinal direction) is 150 to 500 cN, wet paper strength (horizontal direction) is 50 to 300 cN, and water quality is 0.1 to 1.5 seconds. Sanitary tissue paper,
While adding 2.0-20.0 kg / t of a polyamide polyamine epichlorohydrin resin as a wet paper strength enhancer and 0.1-20.0 kg / t of a cationic softening agent to a pulp main material having a freeness of 630 cc or more, 0.1 to 20.0 kg / t of CMC (carboxymethylcellulose) having a degree of etherification of 0.3 to 0.9 or a salt thereof is added,
Home hygiene, characterized in that the calendar type is a soft calender or a metal calender, and the paper is made with a nip line pressure of 7-30 kgf / cm, a nip number of 1-3, and a machine speed of 300-2000 m / min. Tissue paper is provided. Here, the water absorption is a value obtained through the following steps (1) to (5).
(1) Use a digital micropipette, stopwatch, tripod stand as a measuring instrument.
(2) Place two samples as a set on a support with a hole with a diameter of 40 mm or more in the center.
(3) Take distilled water into a digital micropipette and drop 1 drop (0.1 ml) of distilled water onto a test piece from a height of about 10 mm.
(4) The time from when the water droplet contacts the test piece to when the water is completely absorbed and the reflection on the paper surface disappears is measured with a stopwatch in units of 0.01 seconds.
(5) Conduct the test five times, and use the average value obtained by the test procedure to record the first decimal place.
先ず、本請求項1においては、家庭用衛生薄葉紙の抄造に当たり、1枚当たりの米坪を15〜50g/m2とする際に、吸水度が0.1〜1.5秒となるように抄造条件を調整する。なお、本発明における「吸水度」は、後述する試験要領に従った試験値であり、数値が小さいほど吸収性が良好となる。従来の一般的なティッシュペーパーの吸水度は1.8〜3秒程度であり、これと比較すると、本発明に係る衛生薄葉紙の場合には、0.1〜1.5秒の吸水度となっており、テーブルや床などにこぼした液体を迅速に、かつ手際良く拭き取りできるようになっている。 First, in claim 1, when making the sanitary thin paper for household use, when the rice basis weight per sheet is 15 to 50 g / m 2 , the water absorption is 0.1 to 1.5 seconds. Adjust paper making conditions. The “water absorption” in the present invention is a test value according to the test procedure described later, and the smaller the value, the better the absorbency. The water absorption of a conventional general tissue paper is about 1.8 to 3 seconds. Compared with this, in the case of the sanitary thin paper according to the present invention, the water absorption is 0.1 to 1.5 seconds. In addition, liquids spilled on tables and floors can be wiped off quickly and neatly.
前記吸水度の制御は、種々の抄造条件を調整することにより達成することが可能である。主たる因子の一つとして、叩解フリーネス(CSF)を挙げることができる。一般的なティッシュペーパーの場合のフリーネスは600cc未満であるが、本衛生薄葉紙においては、フリーネス(CSF)を630cc以上、好ましくは650cc以上とし、繊維の破壊を抑え吸水性の向上を図るようにし、低叩解によるため強度向上が望めないデメリットは紙力増強剤の添加により補うようにする。なお、叩解フリーネスと紙をミキサーで離解した時の離解フリーネスはほぼ同等となる。また、カレンダー処理条件におけるカレンダー種別、ニップ線圧、ニップ数、マシンスピードなども制御条件である。 The control of the water absorption can be achieved by adjusting various papermaking conditions. One of the main factors is beating freeness (CSF). The freeness in the case of general tissue paper is less than 600 cc, but in the sanitary thin paper, the freeness (CSF) is set to 630 cc or more, preferably 650 cc or more so as to suppress fiber breakage and improve water absorption. The disadvantage that strength cannot be improved due to low beating is compensated by the addition of a paper strength enhancer. The beating freeness and the disintegration freeness when the paper is disintegrated with a mixer are almost the same. Further, the calendar type, the nip line pressure, the number of nips, the machine speed, etc. in the calendar processing conditions are also control conditions.
上記本発明によれば、米坪量が高くても、柔軟で手触り感が良好でありながら、強度特性(湿潤強度、乾燥強度及び表面特性等)が良好で、かつ吸水性に優れた家庭用衛生薄葉紙を得ることができるようになる。 According to the present invention, even if the basis weight of rice is high, it is flexible and has a good touch feeling, but has good strength characteristics (wet strength, dry strength, surface characteristics, etc.) and excellent water absorption. Sanitary thin paper can be obtained.
以下、本発明の実施の形態について図面を参照しながら詳述する。 Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
例えば、広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を所定の割合で配合したパルプスラリー原料により、ロールペーパー、ティッシュペーパー、ちり紙等の家庭用衛生薄葉紙を1枚当たりの米坪が15〜50g/m2となるように抄造するに当たり、各種の操業条件を調整することにより、吸水度が0.1〜1.5秒となるように抄紙するものである。 For example, by using a pulp slurry raw material blended with a predetermined ratio of hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP), a household sanitary thin paper such as roll paper, tissue paper, and dust paper has a rice basis weight of 15 to In making paper so that it may be set to 50 g / m < 2 >, it adjusts various operating conditions and makes paper so that a water absorption may be set to 0.1-1.5 second.
主原料となるパルプは、前記広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)などの化学パルプの他、古紙を脱墨処理して得られる脱墨パルプを用いてもよい。また、これらのパルプは未晒パルプ、晒パルプの状態で用いても良い。また、パルプは叩解又は未叩解の状態で用いてもよいが、フリーネス(CSF)は630cc以上、好ましくは650cc以上とし、繊維の破壊を抑え繊維間のポーラス性を確保するようにする。また、低叩解によるため紙力強度が望めない点については紙力増強剤の添加によってこれを補うようにする。また、カレンダー処理条件におけるカレンダー種別、ニップ線圧、ニップ数、マシンスピードなども制御要因として抄紙を行うようにする。具体的には、カレンダー種別はソフトカレンダー又は金属カレンダーとし、ニップ線圧は7〜30kgf/cm、ニップ数は1〜3、マシンスピードは300〜2000m/分として操業するのが望ましい。 In addition to chemical pulp such as hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP), deinked pulp obtained by deinking waste paper may be used as the main raw material pulp. These pulps may be used in the state of unbleached pulp or bleached pulp. The pulp may be used in a beating or unbeaten state, but the freeness (CSF) is 630 cc or more, preferably 650 cc or more so as to suppress fiber breakage and ensure the porous property between the fibers. Further, the point where the paper strength cannot be expected due to low beating is compensated by the addition of a paper strength enhancer. In addition, paper making is performed by controlling the calendar type, the nip line pressure, the number of nips, the machine speed, etc. in the calendar processing conditions. Specifically, it is desirable that the calendar type is a soft calendar or a metal calendar, the nip linear pressure is 7 to 30 kgf / cm, the number of nips is 1 to 3, and the machine speed is 300 to 2000 m / min.
本発明における「吸水度」は、測定器具としてデジタルマイクロピペット、ストップウォッチ、三脚台を使用し、試料2枚重ねを一組として中央部直径40mm以上の穴のある支持台に置き、デジタルマイクロピペットに蒸留水を取り、約10mmの高さから試験片に蒸留水を1滴(0.1ml)滴下し、水滴が試験片に接触した瞬間から、水が完全に吸収されて紙表面の反射が消えるまでの時間をストップウォッチで0.01秒単位で測定する。試験は5回行い、その平均値を小数点第1位まで記録する試験要領によって得た数値とする。 In the present invention, “water absorption” is measured using a digital micropipette, stopwatch, tripod stand as a measuring instrument, placed on a support base having a hole with a diameter of 40 mm or more as a pair, and a digital micropipette. Take distilled water at a height of about 10 mm and drop 1 drop (0.1 ml) of distilled water onto the test piece from the height of about 10 mm. From the moment when the water droplet touches the test piece, the water is completely absorbed and the reflection on the paper surface is reflected. The time until disappearance is measured with a stopwatch in units of 0.01 seconds. The test is performed 5 times, and the average value is a value obtained by the test procedure for recording to the first decimal place.
前記広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を配合する場合には、針葉樹クラフトパルプを20〜80重量%、広葉樹クラフトパルプを80〜20重量%の割合で配合するのが望ましい。この場合、本発明ではフリーネスを制限している関係上、広葉樹クラフトパルプと針葉樹クラフトパルプを同量とするか、強度増加を強く望む場合は、針葉樹クラフトパルプを多く配合するようにし、柔らかさを強く望む場合には、広葉樹クラフトパルプを多く配合するようにするのが望ましい。 When blending the hardwood kraft pulp (LBKP) and the softwood kraft pulp (NBKP), it is desirable to blend the softwood kraft pulp in a proportion of 20 to 80% by weight and the hardwood kraft pulp in a proportion of 80 to 20% by weight. In this case, since freeness is limited in the present invention, if the hardwood kraft pulp and the softwood kraft pulp are the same amount, or if it is strongly desired to increase the strength, a large amount of softwood kraft pulp is added, and the softness is increased. If strongly desired, it is desirable to add more hardwood kraft pulp.
本発明に係るティッシュペーパーの1枚当たりの米坪は、15〜50g/m2、好ましくは18〜30g/m2とされる。従来一般のティッシュペーパーの坪量は11〜16g/m2であることを考慮すると、かなり厚手のものとなる。米坪が15g/m2未満の場合には、拭き取りに適した十分な厚み、丈夫さが得られない。また、米坪が50g/m2を超える場合には、拭き取りに適したしなやかさが得られない。このティッシュペーパーは単体シートとして、または2〜4枚重ねとして提供される。 The rice paper weight of the tissue paper according to the present invention is 15 to 50 g / m 2 , preferably 18 to 30 g / m 2 . Considering that the basis weight of conventional tissue paper is 11 to 16 g / m 2 , the tissue paper is considerably thick. When the rice tsubo is less than 15 g / m 2 , sufficient thickness and strength suitable for wiping cannot be obtained. On the other hand, when the weight per square meter exceeds 50 g / m 2 , the flexibility suitable for wiping cannot be obtained. This tissue paper is provided as a single sheet or as a stack of 2-4 sheets.
ティッシュペーパーの抄造に当たっては、湿潤紙力増強剤の添加により湿潤紙力の向上を図るようにする。一般紙の場合には、例えば尿素ホルムアルデヒド樹脂、メラミンホルムアルデヒド樹脂、ポリアミドポリアミンエピクロルヒドリン樹脂等の湿潤紙力増強剤が用いられるが、ティッシュペーパーの場合には人体への影響を考慮してホルムアルデヒド樹脂は避け、ポリアミドポリアミンエピクロルヒドリン樹脂が主として用いられる。添加量は、乾燥重量で2.0〜20.0kg/t、好ましくは2.5〜5.0kg/tとするのが望ましい。添加量が2.0kg/t未満の場合は、十分な湿潤紙力強度が得られず、20.0kg/tを超える場合にはシートが硬く成りすぎて拭取り性が低下するようになる。 In making tissue paper, the wet paper strength is improved by adding a wet paper strength enhancer. In the case of general paper, wet paper strength enhancers such as urea formaldehyde resin, melamine formaldehyde resin, and polyamide polyamine epichlorohydrin resin are used, but in the case of tissue paper, formaldehyde resin should be avoided in consideration of effects on the human body. Polyamide polyamine epichlorohydrin resin is mainly used. The addition amount is 2.0 to 20.0 kg / t, preferably 2.5 to 5.0 kg / t in terms of dry weight. When the addition amount is less than 2.0 kg / t, sufficient wet paper strength cannot be obtained, and when it exceeds 20.0 kg / t, the sheet becomes too hard and the wiping property is lowered.
また、シートには前記湿潤紙力剤と共に、柔らかさや手触り感をもたせるために、紙用柔軟剤を添加することができる。この紙用柔軟剤としては、例えば脂肪酸エステル系柔軟剤(米国特許第3,296,065号明細書)、第4級アンモニウム塩型カチオン活性剤(特開昭48−22701号公報)、ウレタンアルコール若しくはその塩、またはカチオン化物(特開昭60−139897号公報)、非陽イオン系界面活性剤(特開平2−99690号公報、同2−99691号公報)、ポリリン酸塩(特開平2−36288号公報)、ポリシロキサン(特開平2−224626号公報、同3−900号公報)などを挙げることができる。これらの中でも、カチオン系柔軟剤を使用するのが望ましい。その添加量は、0.1〜20.0kg/t、好ましくは0.5〜5.0kg/tとするのが望ましい。添加量が0.1kg/t未満の場合は、風合いを向上させ、柔らかくする十分な効果が得られない。また、20.0kg/tを超える場合には、乾燥紙力の低下が顕著となり拭き取り時に破れやすくなる。 In addition to the wet paper strength agent, a softening agent for paper can be added to the sheet in order to give a soft feeling and a hand feeling. Examples of the paper softener include fatty acid ester softener (US Pat. No. 3,296,065), quaternary ammonium salt type cationic activator (Japanese Patent Laid-Open No. 48-22701), urethane alcohol or a salt thereof, Or a cationized product (JP-A-60-139897), a non-cationic surfactant (JP-A-2-99690, JP-A-2-99691), polyphosphate (JP-A-2-36288) And polysiloxane (JP-A-2-224626 and JP-A-3-900). Among these, it is desirable to use a cationic softening agent. The addition amount is 0.1 to 20.0 kg / t, preferably 0.5 to 5.0 kg / t. When the addition amount is less than 0.1 kg / t, a sufficient effect of improving the texture and softening cannot be obtained. Moreover, when it exceeds 20.0 kg / t, the fall of dry paper force becomes remarkable and it becomes easy to tear at the time of wiping off.
さらに、本衛生薄葉紙においては、前記湿潤紙力剤、柔軟剤と共に、若しくはこれら添加剤の1種と共に、CMC(カルボキシメチルセルロース)又はその塩を添加するのが望ましい。CMC又はその塩を原料パルプに添加した場合、乾燥紙力剤として働くと同時に、湿潤紙力剤(ポリアミドポリアミンエピクロルヒドリン樹脂)がスラリー中に存在している場合には、これと結合して湿潤紙力を向上させるようになる。また、スラリー中にカチオン系柔軟剤が存在している場合にはこれと結合してパルプに定着し、柔軟性(フレキシビリティ)を向上させるようになる。また、一般的な湿潤紙力剤はカチオン性が高く微細繊維(アニオン性)を凝縮して紙を硬くする性質があるが、アニオン性のCMCが存在すると、微細繊維の凝集は相対的に抑制され、紙が硬くなり難い。 Furthermore, in the sanitary thin paper, it is desirable to add CMC (carboxymethylcellulose) or a salt thereof together with the wet paper strength agent, the softening agent, or one of these additives. When CMC or a salt thereof is added to the raw material pulp, it acts as a dry paper strength agent, and at the same time, when a wet strength agent (polyamide polyamine epichlorohydrin resin) is present in the slurry, it is combined with the wet paper strength agent. To improve power. Further, when a cationic softening agent is present in the slurry, it is combined with it and fixed on the pulp, thereby improving the flexibility. In addition, general wet paper strength agents are highly cationic and have the property of condensing fine fibers (anionic) to harden the paper, but when anionic CMC is present, aggregation of fine fibers is relatively suppressed. The paper is hard to harden.
ティッシュペーパーの抄紙機としては、丸網、短網、ツインワイヤー等の抄紙機にヤンキー乾燥機を組み合わせたごく一般的に使用されるものとすることができる。 As a paper machine for tissue paper, a paper machine such as a round net, a short net, or a twin wire can be used generally in combination with a Yankee dryer.
本発明に従って抄紙された衛生薄葉紙1枚当たりの乾燥紙力(縦方向)は400〜1400cN、好ましくは500〜1100cN、乾燥紙力(横方向)は200〜500cN、好ましくは250〜400cNとされる。乾燥紙力が上記数値未満の場合には拭き取りの丈夫さが十分ではなく、上記数値を超える場合には拭き取り時の柔軟性が十分でない。 The dry paper strength (longitudinal direction) per sanitary thin paper made according to the present invention is 400 to 1400 cN, preferably 500 to 1100 cN, and the dry paper strength (lateral direction) is 200 to 500 cN, preferably 250 to 400 cN. . When the dry paper strength is less than the above value, the wiping strength is not sufficient, and when it exceeds the above value, the flexibility at the time of wiping is not sufficient.
また、衛生薄葉紙1枚当たりの湿潤紙力(縦方向)は150〜500cN、好ましくは250〜400cN、湿潤紙力(横方向)は50〜300cN、好ましくは100〜250cNとされる。湿潤紙力が上記数値未満の場合は湿潤時における丈夫さが十分ではなく、上記数値を超える場合には湿潤時の拭き取り時の柔軟性が十分ではない。 Further, the wet paper strength (longitudinal direction) per sanitary thin paper is 150 to 500 cN, preferably 250 to 400 cN, and the wet paper strength (lateral direction) is 50 to 300 cN, preferably 100 to 250 cN. When the wet paper strength is less than the above value, the strength when wet is not sufficient, and when it exceeds the above value, the flexibility during wiping when wet is insufficient.
一方で、{(湿潤紙力(縦方向)×湿潤紙力(横方向))}1/2/ソフトネスの値が100〜3000、好ましくは300〜1200であることが望ましい。上記値が100未満の場合は拭き取り時の柔らかさが十分でなく、3000を超える場合には柔らかすぎて拭き取り時に安心感が得られない。 On the other hand, the value of {(wet paper strength (vertical direction) × wet paper strength (lateral direction))} 1/2 / softness is 100 to 3000, preferably 300 to 1200. When the above value is less than 100, the softness at the time of wiping is not sufficient, and when it exceeds 3000, it is too soft to provide a sense of security at the time of wiping.
前記ソフトネスは、JIS L1096 ハンドルオーメーター法により準拠した測定方法によって測定する。具体的には、ペーパーシート(100×100mm)を一定の隙間(5mm)に押し入れるのに必要な仕事量を測定する原理のハンドルオーメーターによる測定値を以下の手順で得る。
(1)ペーパーシートを100×100mmに裁断する。
(2)ペーパーシートは加圧板が試料の中心を折り曲げるように受板の上に置く。
(3)試験は縦方向、横方向各4回測定する。
(4)縦横の平均値
・縦横各平均値
・ソフトネス(cN)=0.9807×(縦のソフトネス(g)×横のソフトネス(g))1/2
The softness is measured by a measuring method based on the JIS L1096 handle ohmmeter method. Specifically, a measurement value by a handle ohmmeter based on the principle of measuring a work amount required to push a paper sheet (100 × 100 mm) into a certain gap (5 mm) is obtained by the following procedure.
(1) Cut the paper sheet into 100x100mm.
(2) Place the paper sheet on the receiving plate so that the pressure plate bends the center of the sample.
(3) The test is measured four times in the vertical and horizontal directions.
(4) Vertical and horizontal average values, vertical and horizontal average values, softness (cN) = 0.9807 x (vertical softness (g) x horizontal softness (g)) 1/2
他方で、前記(湿潤紙力(縦方向)×湿潤紙力(横方向))/(乾燥紙力(縦方向)×乾燥紙力(横方向))の値は0.15〜0.25、好ましくは0.16〜0.20であることが望ましい。上記値が0.15未満の場合には拭き取りの湿潤紙力が十分ではなく、0.25を超える場合は拭き取り時に強度が強すぎて拭き取り時の柔軟性が悪くなる。 On the other hand, the value of (wet paper strength (vertical direction) × wet paper strength (horizontal direction)) / (dry paper strength (vertical direction) × dry paper strength (horizontal direction)) is 0.15 to 0.25, Preferably it is 0.16-0.20. When the above value is less than 0.15, the wet paper strength for wiping is not sufficient, and when it exceeds 0.25, the strength is too strong at the time of wiping and the flexibility at the time of wiping is deteriorated.
次いで、シートの表面特性に関して、摩擦係数の平均偏差(摩擦子を移動させたときの表面粗さの変動:MMD)は10.0〜20.0、好ましくは10.0〜16.5とするのが望ましい。前記MMDは、カトーテック株式会社製「摩擦感テスター KESSE」を用いて測定した値である。測定に際しては、図1に示されるように、直径0.5mmのピアノ線を10本隣接させ、先端の曲率半径が0.25mmの単位膨出部を隣接して有し、全幅が5mmの連続した接触面を有し、その接触面の長さは5mmである摩擦子を、紙試料に50gの接触圧で接触させながら、移動方向に20g/cmの張力を紙試料に与えつつ、0.1cm/秒の速度で2cm移動させたときの摩擦係数を測定し、この摩擦係数を摩擦距離(移動距離=2cm)で除した値とする。 Next, regarding the surface characteristics of the sheet, the average deviation of the friction coefficient (variation of surface roughness when the friction element is moved: MMD) is 10.0 to 20.0, preferably 10.0 to 16.5. Is desirable. The MMD is a value measured using “Friction Tester KESSE” manufactured by Kato Tech Co., Ltd. In the measurement, as shown in FIG. 1, ten piano wires having a diameter of 0.5 mm are adjacent to each other, a unit bulging portion having a radius of curvature of the tip is adjacent to 0.25 mm, and the total width is 5 mm. While a friction element having a continuous contact surface and a contact surface length of 5 mm is brought into contact with the paper sample at a contact pressure of 50 g, a tension of 20 g / cm is applied to the paper sample in the moving direction. Measure the friction coefficient when moved 2 cm at a speed of 1 cm / sec, and divide this friction coefficient by the friction distance (movement distance = 2 cm).
前記MMDが10.0未満の場合は、拭き取り時の摩擦が小さく、拭き取りに適さないシートとなり、20.0を超える場合には、表面性が粗くガサガサしてフェイシャル用途に適さないものとなる。 When the MMD is less than 10.0, the friction at the time of wiping is small and the sheet is not suitable for wiping. When the MMD is more than 20.0, the surface property is rough and the sheet is not suitable for facial use.
次に、実施例を挙げて本発明を具体的に説明するが、本発明はこれらの実施例に限定されない。なお、実施例中の部、%は特に断らない限り、それぞれ重量部、重量%を示す。 Next, the present invention will be specifically described with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise indicated, the part and% in an Example show a weight part and weight%, respectively.
(比較例3)
広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を50:50の比率で配合したパルプスラリーをフリーネス670mlに調整し、湿潤紙力剤としてポリアミドポリアミンエピクロルヒドリン樹脂を4.0kg/t添加するとともに、カチオン性柔軟剤を1.0kg/t添加し、丸網抄紙機、ヤンキー乾燥機にて米坪26.0g/m2の衛生薄葉紙(ティッシュペーパー)を製造した。
(Comparative Example 3)
A pulp slurry containing hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP) in a ratio of 50:50 was adjusted to 670 ml of freeness, and polyamide polyamine epichlorohydrin resin as a wet paper strength agent was added at 4.0 kg / t, A cationic softener was added at 1.0 kg / t, and sanitary thin paper (tissue paper) having a weight of 26.0 g / m 2 was produced with a round net paper machine and a Yankee dryer.
(比較例4)
カチオン系柔軟剤を1.3kg/tとした以外は、比較例3と同様として衛生薄葉紙を製造した。
(Comparative Example 4)
A sanitary thin paper was produced in the same manner as Comparative Example 3 except that the cationic softening agent was 1.3 kg / t.
(比較例5)
広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を70:30の比率とし、湿潤紙力剤を3.0kg/tとし、カチオン系柔軟剤を4.5kg/tとした以外は比較例3と同様として衛生薄葉紙を製造した。
(Comparative Example 5)
Comparative Example 3 except that hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP) were in a ratio of 70:30, wet paper strength was 3.0 kg / t, and cationic softener was 4.5 kg / t. A sanitary thin paper was produced in the same manner.
(実施例1)
カチオン系柔軟剤を3.0kg/tとし、CMCを2.0kg/t添加した以外は、比較例3と同様として衛生薄葉紙を製造した。
Example 1
A sanitary thin paper was produced in the same manner as in Comparative Example 3, except that the cationic softening agent was 3.0 kg / t and CMC was added 2.0 kg / t.
(比較例1)
広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を40:60の比率で配合したパルプスラリーをフリーネス450mlに調整し、湿潤紙力剤としてポリアミドポリアミンエピクロルヒドリン樹脂を1.7kg/t添加するとともに、カチオン性柔軟剤を2.8kg/t添加し、丸網抄紙機、ヤンキー乾燥機にて米坪12.2g/m2の衛生薄葉紙(ティッシュペーパー)を製造した。
(Comparative Example 1)
A pulp slurry containing hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP) in a ratio of 40:60 was adjusted to 450 ml freeness, and 1.7 kg / t of polyamide polyamine epichlorohydrin resin was added as a wet paper strength agent. 2.8 kg / t of a cationic softening agent was added, and sanitary thin paper (tissue paper) having a basis weight of 12.2 g / m 2 was produced using a round net paper machine and a Yankee dryer.
(比較例2)
広葉樹クラフトパルプ(LBKP)及び針葉樹クラフトパルプ(NBKP)を50:50の比率で配合したパルプスラリーをフリーネス590mlに調整した以外は、比較例1と同様として衛生薄葉紙を製造した。
(Comparative Example 2)
A sanitary thin paper was produced in the same manner as Comparative Example 1 except that the pulp slurry containing hardwood kraft pulp (LBKP) and softwood kraft pulp (NBKP) in a 50:50 ratio was adjusted to 590 ml of freeness.
これらの衛生薄葉紙(ティッシュペーパー)の各種試験結果は下表1のとおりである。 The various test results of these sanitary thin paper (tissue paper) are shown in Table 1 below.
なお、表中、乾燥紙力はJIS P 8113(引張特性試験方法)に従って試験を行い、湿潤紙力はJIS P 8135(湿潤引張強さ試験方法)に従って試験を行った。また、官能評価は、男女5人づつにより、非常に良い:◎、良い:○、普通:△、劣る:×の4段階で評価した。 In the table, dry paper strength was tested according to JIS P 8113 (tensile property test method), and wet paper strength was tested according to JIS P 8135 (wet tensile strength test method). In addition, sensory evaluation was performed by four men and women in four stages: very good: ◎, good: ○, normal: △, inferior: ×.
Claims (1)
フリーネスが630cc以上としたパルプ主原料に、湿潤紙力増強剤としてポリアミドポリアミンエピクロルヒドリン樹脂を2.0〜20.0kg/t、カチオン系柔軟剤を0.1〜20.0kg/t添加するとともに、エーテル化度0.3〜0.9のCMC(カルボキシメチルセルロース)又はその塩を0.1〜20.0kg/t添加し、
カレンダー処理条件におけるカレンダー種別がソフトカレンダー又は金属カレンダーとし、ニップ線圧が7〜30kgf/cm、ニップ数が1〜3、マシンスピードが300〜2000m/分として抄紙したことを特徴とする家庭用衛生薄葉紙。
ここで、前記吸水度は次記(1)〜(5)の工程を経て得た値である。
(1)測定器具としてデジタルマイクロピペット、ストップウォッチ、三脚台を使用する。
(2)試料2枚重ねを一組として中央部直径40mm以上の穴のある支持台に置く。
(3)デジタルマイクロピペットに蒸留水を取り、約10mmの高さから試験片に蒸留水を1滴(0.1ml)滴下する。
(4)水滴が試験片に接触した瞬間から、水が完全に吸収されて紙表面の反射が消えるまでの時間をストップウォッチで0.01秒単位で測定する。
(5)試験は5回行い、その平均値を小数点第1位まで記録する試験要領によって得た数値とする。 US basis weight per sheet is 15 to 50 g / m 2 , dry paper strength (longitudinal direction) is 400 to 1400 cN, dry paper strength (lateral direction) is 200 to 500 cN, and wet paper strength (vertical direction) is 150 to A hygienic thin paper for home use having a paper quality of 500 cN, wet paper strength (lateral direction) of 50 to 300 cN, and water absorption of 0.1 to 1.5 seconds,
While adding 2.0-20.0 kg / t of a polyamide polyamine epichlorohydrin resin as a wet paper strength enhancer and 0.1-20.0 kg / t of a cationic softening agent to a pulp main material having a freeness of 630 cc or more, 0.1 to 20.0 kg / t of CMC (carboxymethylcellulose) having a degree of etherification of 0.3 to 0.9 or a salt thereof is added,
Home hygiene, characterized in that the calendar type is a soft calender or a metal calender, and the paper is made with a nip line pressure of 7-30 kgf / cm, a nip number of 1-3, and a machine speed of 300-2000 m / min. Tissue paper.
Here, the water absorption is a value obtained through the following steps (1) to (5).
(1) Use a digital micropipette, stopwatch, tripod stand as a measuring instrument.
(2) Place two samples as a set on a support with a hole with a diameter of 40 mm or more in the center.
(3) Take distilled water into a digital micropipette and drop 1 drop (0.1 ml) of distilled water onto a test piece from a height of about 10 mm.
(4) The time from when the water droplet contacts the test piece to when the water is completely absorbed and the reflection on the paper surface disappears is measured with a stopwatch in units of 0.01 seconds.
(5) Conduct the test five times, and use the average value obtained by the test procedure to record the first decimal place.