JP2012030125A - Method for producing household sanitary tissue - Google Patents

Method for producing household sanitary tissue Download PDF

Info

Publication number
JP2012030125A
JP2012030125A JP2011249729A JP2011249729A JP2012030125A JP 2012030125 A JP2012030125 A JP 2012030125A JP 2011249729 A JP2011249729 A JP 2011249729A JP 2011249729 A JP2011249729 A JP 2011249729A JP 2012030125 A JP2012030125 A JP 2012030125A
Authority
JP
Japan
Prior art keywords
paper
chemical solution
active ingredient
roll
weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2011249729A
Other languages
Japanese (ja)
Other versions
JP5425867B2 (en
Inventor
Akira Hirasawa
朗 平沢
Saeko Ito
佐絵子 伊藤
Hiroshi Ono
浩 大野
Mitsuru Ishibashi
満 石橋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Daio Paper Corp
Original Assignee
Daio Paper Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Daio Paper Corp filed Critical Daio Paper Corp
Priority to JP2011249729A priority Critical patent/JP5425867B2/en
Publication of JP2012030125A publication Critical patent/JP2012030125A/en
Application granted granted Critical
Publication of JP5425867B2 publication Critical patent/JP5425867B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

PROBLEM TO BE SOLVED: To provide a household sanitary tissue exhibiting improved target texture (softness), moisture-holding properties and the like, with a reduced amount of medical fluid applied thereto, by the inhibition of the elongation of sheet thereof, the reduction of the basis weight thereof, and a decrease of stiffness thereof.SOLUTION: In an interfolder, when raw paper prepared from a pulp fiber is wound by winding rolls 1, 2 with prescribed width and continuous sheets 10, 20 are rewound from the winding rolls respectively, and then, folded and piled by a folding and piling means 50, prior to the folding and piling, medical fluid is continuously applied onto the target sheets by roll transfer by means of roll transfer devices 33, 34 and 43, 44 for applying the medical fluid onto the target sheets.

Description

本発明は、ドライタイプのティシュペーパーなどの家庭用衛生薄葉紙の製造方法に関する。   The present invention relates to a method for producing household sanitary thin paper such as dry type tissue paper.

近時、いわゆるローション薬液を含有させることにより肌触りを柔らかくした、汎用のティシュペーパーに対し高級タイプのティシュペーパー(ウエットタイプのものに対し、ドライタイプのティシュペーパーとして呼ばれている)が市販され、繰り返し鼻をかんでも肌がヒリヒリし難い、または鼻が赤くなり難いとして人気を呼んでいる。   Recently, a high-quality tissue paper (called a dry-type tissue paper for a wet type), which is soft to the touch by containing a so-called lotion chemical, is commercially available, It is popular because it makes it difficult for the skin to tingle even when the nose is repeatedly pinched, or the nose does not turn red easily.

本出願人は、さらに改良された家庭用衛生薄葉紙についていくつかの提案をなしている(特許文献1及び特許文献2)。
たとえば、特許文献1及び2においては、柔軟剤や保湿剤を含む薬液を基剤紙に対し46mg/cm3以上含有させるようにしている。
The present applicant has made several proposals for further improved household sanitary thin paper (Patent Document 1 and Patent Document 2).
For example, in Patent Documents 1 and 2, a chemical solution containing a softening agent and a humectant is contained in a base paper at 46 mg / cm 3 or more.

いわゆるローション薬液の塗布に際し、スプレー塗布を採用できるが、充分なる塗布量を得がたい。しかも、可能な限り充分なる塗布量を得るためには、プライ加工後でインターフォルダにかける前に、オフラインで薬液の塗布を行う必要がある。   Spray application can be employed for applying a so-called lotion chemical, but it is difficult to obtain a sufficient application amount. Moreover, in order to obtain a coating amount as much as possible, it is necessary to apply the chemical solution off-line before applying to the interfolder after ply processing.

しかし、オフラインでの薬液の塗布方法を採ると、薬液塗布によって、インターフォルダにかける前での巻き取り段階などにおいてシートの伸びが生じるので、原紙の米坪を高める必要がある。シートの伸びは、オフラインでのロール塗布においても生じる。   However, when an off-line method for applying a chemical solution is employed, since the sheet is stretched by a chemical solution application at a winding stage before being applied to an interfolder, it is necessary to increase the rice paper weight of the base paper. Sheet elongation also occurs in off-line roll coating.

原紙の米坪を高めると、パルプ使用量の増大に伴いコスト高の要因となるばかりでなく、紙のコシが大きくなり柔軟性を阻害し、しかもこれを回避するために柔軟剤などの使用量を増す必要があるなどの悪循環に陥る。
特開2001−164385号公報 特開2003−164386公報
Increasing the base weight of the base paper not only causes a cost increase with an increase in the amount of pulp used, but also increases the stiffness of the paper, impairs flexibility and uses softeners to avoid this. Fall into a vicious circle.
JP 2001-164385 A JP 2003-164386 A

したがって、本発明の課題は、シートの伸びを防止し、米坪を低減させ、紙のコシが小さいものとすることで、薬液塗布量を低減しながらも、目的の肌触り性(風合い)を高めたり保湿性などの特性を示す家庭用衛生薄葉紙、及びその家庭用衛生薄葉紙を得ることができる家庭用衛生薄葉紙の製造方法を提供することにある。   Therefore, the object of the present invention is to prevent the sheet from being stretched, to reduce the weight of the paper, and to reduce the stiffness of the paper, thereby reducing the amount of chemical solution applied and improving the desired touch (texture). Another object of the present invention is to provide a household sanitary thin paper exhibiting characteristics such as moisturizing properties and a method for producing a home sanitary thin paper from which the home sanitary thin paper can be obtained.

上記課題を解決した本発明は以下のとおりである。
<請求項1項記載の発明>
インターフォルダにおいて、パルプ繊維を抄造した原紙を所定の幅で巻き取った巻取ロールから連続シートをそれぞれ巻き戻して、これらを折り畳み積み重ねて製品化する家庭用衛生薄葉紙の製造方法において、
抄造工程で前記原紙に対して、有効成分として、湿潤紙力剤、柔軟剤およびカルボキシメチルセルロースの少なくとも一種を添加剤として予め添加しておき、
前記インターフォルダにおける巻き戻しから折り畳み積み重ね工程の間で、前記連続シートに、有効成分として前記添加剤とは別の保湿性薬液をpHを5.0〜6.0に調整してグラビアロールによるロール転写で連続的に塗布し、その後にプレス装置により前記薬液を含浸させて、シート単位容積当たりの薬液含有量を12〜45mg/cm3とする、ことを特徴とする家庭用衛生薄葉紙の製造方法。
<請求項2記載の発明>
有効成分における湿潤紙力剤、柔軟剤およびカルボキシメチルセルロースの少なくとも一種の比率を3.0〜4.5重量%とし、
有効成分における薬液の比率を95.5〜97.0重量%とする、請求項1記載の家庭用衛生薄葉紙の製造方法。
The present invention that has solved the above problems is as follows.
<Invention of Claim 1>
In the inter folder, in the manufacturing method of household sanitary thin paper, each continuous sheet is rewound from a winding roll obtained by winding a base paper made of pulp fiber with a predetermined width, and these are folded and stacked to produce a product.
For the base paper in the paper making process, as an active ingredient, at least one of wet paper strength agent, softener and carboxymethylcellulose is added in advance as an additive,
A roll by a gravure roll by adjusting a pH of a moisturizing chemical solution different from the additive as an active ingredient to 5.0 to 6.0 as an active ingredient between unwinding and folding stacking steps in the interfolder A method for producing a sanitary thin paper for home use, characterized in that the chemical solution is continuously applied by transfer and then impregnated with the chemical solution by a pressing device so that the chemical solution content per sheet unit volume is 12 to 45 mg / cm 3. .
<Invention of Claim 2>
The ratio of at least one of wet paper strength agent, softener and carboxymethyl cellulose in the active ingredient is 3.0 to 4.5% by weight,
The manufacturing method of the household sanitary thin paper of Claim 1 which makes the ratio of the chemical | medical solution in an active ingredient 95.5 to 97.0 weight%.

(作用効果)
本発明は、インターフォルダにおいて、巻き戻しから折り畳み積み重ね工程の間で、連続シートにいわゆるローション薬液をロール転写で連続的に塗布するものである。ロール転写により薬液を塗布すると、スプレー塗布による場合より、基材紙への薬液の塗布量を多くすることができる。また、インターフォルダにおいてオンライン塗布を行うので、紙の伸びを生じることがなく、米坪を低いものとすることができ、紙のコシが小さいあるいは風合いに優れたものとすることができ、もって、少ない薬液塗布量であっても柔軟性に富むものを得ることができる。この米坪を低く、薬液塗布量を少なくすることは経済性に優れることを意味する。
また、薬液のロール転写塗布をグラビアロールにより行うことにより、凹凸のないロールの場合に比較して、薬液塗布量を多くすることができる。
なお、本発明のローション薬液としては、主に、肌触り性(風合い)を高めたり、保湿性を高め、パルプ繊維の肌への刺激を和らげるあるいは潤い感を高めることを主眼とするものである。
(Function and effect)
In the interfolder, a so-called lotion chemical solution is continuously applied to a continuous sheet by roll transfer between unwinding and folding and stacking processes. When the chemical solution is applied by roll transfer, the amount of the chemical solution applied to the base paper can be increased as compared with the case of spray coating. In addition, since the online application is performed in the interfolder, the paper does not stretch, the basis weight of the paper can be lowered, the paper is less stiff or has an excellent texture, Even with a small amount of chemical solution applied, a product with high flexibility can be obtained. Lowering the rice tsubo and reducing the amount of the chemical solution applied means better economy.
Moreover, by performing roll transfer application of the chemical solution with a gravure roll, the amount of the chemical solution applied can be increased as compared to a roll without unevenness.
The lotion chemical solution of the present invention is mainly intended to increase the touch (texture), increase the moisture retention, relieve the stimulation of the pulp fiber skin, or increase the moisturizing feeling.

原紙の抄造工程において、前記の本発明の対象薬液以外の別種の添加剤、たとえば界面活性剤からなる柔軟剤、でんぷんやデキストリンなどの湿潤紙力剤、カルボキシメチルセルロースなどの一種または二種以上を添加すると、本発明の対象薬液と相俟って風合いを改善できる。一方、すべての液をインターフォルダにおいてオンライン塗布することも想定できるが、一度に紙力低下が起きる傾向があり、実生産を行う上で断紙が多発し、これを防止するために、添加剤については先に添加するのが好ましいのである。
添加剤として、湿潤紙力剤、柔軟剤及びカルボキシメチルセルロースの少なくとも一種を使用するのが望ましい。この理由は、湿潤紙力剤及び柔軟剤はカチオン性であるのに対し、カルボキシメチルセルロースはアニオン性である。その結果、アニオン性であるパルプ繊維に対し、カチオン性である湿潤紙力剤及び柔軟剤が吸着する際に、アニオン性であるカルボキシメチルセルロースが吸着媒体となり、繊維に確実に吸着させ、湿潤紙力剤及び柔軟剤が元来もつ機能を発揮させることができる。しかも、カルボキシメチルセルロース自体が乾燥紙力を向上させるべく機能する。
In the paper making process of the base paper, other types of additives other than the above-described chemical solution of the present invention, for example, a softening agent comprising a surfactant, a wet paper strength agent such as starch or dextrin, or one or more of carboxymethyl cellulose are added. Then, the texture can be improved in combination with the target drug solution of the present invention. On the other hand, it can be assumed that all liquids are applied on-line in the interfolder, but there is a tendency for paper strength to drop at once. Is preferably added first.
As an additive, it is desirable to use at least one of a wet paper strength agent, a softening agent, and carboxymethyl cellulose. This is because wet paper strength and softeners are cationic, whereas carboxymethyl cellulose is anionic. As a result, when the cationic wet paper strength agent and softening agent are adsorbed to the anionic pulp fiber, the anionic carboxymethyl cellulose becomes an adsorption medium, which is reliably adsorbed on the fiber, and the wet paper strength. The functions inherent to the agent and softener can be exhibited. Moreover, carboxymethylcellulose itself functions to improve the dry paper strength.

<本発明により製造される家庭用衛生薄葉紙の発明>
原紙の1プライ当たりの米坪が10〜25g/m2であり、薬液のシート単位容積当たりの含有量が12〜45mg/cm3であり、製品におけるJIS P8111で規定する条件で調湿し、JIS P8127で測定した水分率が10.0〜20.0%であり、製品におけるソフトネスが0.5〜1.0gであり、製品におけるオイルKES肌触り指数が6.5以下であり、
80〜100重量%の有効成分を含むとともに、その有効成分として前記薬液を95.5〜97.0重量%、ならびに湿潤紙力剤、柔軟剤およびカルボキシメチルセルロースの少なくとも一種を3.0〜4.5重量%含む液を原紙に添加させてなる、
ことを特徴とする家庭用衛生薄葉紙。
<Invention of Household Sanitary Thin Paper Manufactured by the Present Invention>
The basis weight per ply of the base paper is 10 to 25 g / m 2 , the content per unit volume of the chemical solution is 12 to 45 mg / cm 3 , and the humidity is adjusted under the conditions specified in JIS P8111 in the product. The moisture content measured by JIS P8127 is 10.0-20.0%, the softness in the product is 0.5-1.0 g, and the oil KES touch index in the product is 6.5 or less,
80 to 100% by weight of the active ingredient, and 95.5 to 97.0% by weight of the chemical solution as the active ingredient, and at least one of a wet paper strength agent, a softening agent and carboxymethylcellulose is 3.0 to 4. A liquid containing 5% by weight is added to the base paper.
A sanitary thin paper for household use.

(作用効果)
薬液のシート単位容積当たりの含有量を12〜45mg/cm3と少ないものでありながら、原紙の米坪(1プライ当り)が10〜25g/m2と低いものであることから紙のコシ(剛性)が小さいので、柔軟性感及び風合いに優れたものとなる。そして、水分率が高いのでしっとり感を与えるものとなる。また、本発明によって、低いソフトネスのものを得ることができる。さらに、本発明によって、風合い及び肌触りに優れたものを得ることができる。
添加剤として、湿潤紙力剤、柔軟剤及びカルボキシメチルセルロースの少なくとも一種を使用するのが望ましい。この理由は、湿潤紙力剤及び柔軟剤はカチオン性であるのに対し、カルボキシメチルセルロースはアニオン性である。その結果、アニオン性であるパルプ繊維に対し、カチオン性である湿潤紙力剤及び柔軟剤が吸着する際に、アニオン性であるカルボキシメチルセルロースが吸着媒体となり、繊維に確実に吸着させ、湿潤紙力剤及び柔軟剤が元来もつ機能を発揮させることができる。しかも、カルボキシメチルセルロース自体が乾燥紙力を向上させるべく機能する。
(Function and effect)
Although the content of the chemical solution per sheet unit volume is as small as 12 to 45 mg / cm 3 , the base weight of the base paper (per ply) is as low as 10 to 25 g / m 2. Since (rigidity) is small, it has excellent flexibility and texture. And since the moisture content is high, it gives a moist feeling. In addition, the present invention can obtain a low softness. Furthermore, according to the present invention, it is possible to obtain an excellent texture and touch.
As an additive, it is desirable to use at least one of a wet paper strength agent, a softening agent, and carboxymethyl cellulose. This is because wet paper strength and softeners are cationic, whereas carboxymethyl cellulose is anionic. As a result, when the cationic wet paper strength agent and softening agent are adsorbed to the anionic pulp fiber, the anionic carboxymethyl cellulose becomes an adsorption medium, which is reliably adsorbed on the fiber, and the wet paper strength. The functions inherent to the agent and softener can be exhibited. Moreover, carboxymethylcellulose itself functions to improve the dry paper strength.

本発明によれば、シートの伸びを防止し、米坪を低減させ、紙のコシが小さいものとすることで、薬液塗布量を低減しながらも、目的の肌触り性(風合い)や保湿性などの特性を示す家庭用衛生薄葉紙を得ることができる。   According to the present invention, the elongation of the sheet is prevented, the rice paper weight is reduced, and the paper stiffness is small, so that the desired touch (texture), moisture retention, etc. are achieved while reducing the amount of chemical solution applied. It is possible to obtain a household sanitary thin paper exhibiting these characteristics.

以下本発明を実施するための最良の形態を示しながら本発明をさらに詳説する。
本発明は、ドライタイプのティシュペーパーなどの家庭用衛生薄葉紙を提供するものである。したがって、水分率としては100%未満であり、通常は80%以下であり、工場出荷段階では工場内の湿度に依存するが、使用時点(取り出し段階)では大気中湿度にほぼ対応した水分率を有するものである。好ましい水分率は、通常の紙製家庭用衛生薄葉紙容器内に収納・未開封時において、10〜20%、特に10〜15%(JIS P8111で規定する条件で調湿し、JIS P8127で測定した水分率)である。
Hereinafter, the present invention will be described in more detail while showing the best mode for carrying out the present invention.
The present invention provides household sanitary thin paper such as dry-type tissue paper. Therefore, the moisture content is less than 100%, usually 80% or less, and depends on the humidity in the factory at the factory shipment stage. However, at the time of use (takeout stage), the moisture content almost corresponds to the atmospheric humidity. It is what you have. The preferred moisture content is 10 to 20%, particularly 10 to 15% (measured according to JIS P8111 and measured by JIS P8127) when stored in an ordinary paper household sanitary thin paper container and unopened. Moisture content).

<製造形態>
まず、本発明に係る製造方法を説明する。
箱詰型ティッシュペーパーの製造にあたり、抄紙装置においてパルプ繊維(望ましくは古紙パルプを含まないバージンパルプ100%のパルプ繊維)から薄葉紙を抄造し、必要によりクレープを施し、カレンダー処理を施した上で、これを巻き取り一次原反ロール(一般にジャンボロールともいわれている)を製造し、次いで図示しないが、この一次原反ロールを公知のプライマシンにセットし、複数の一次原反ロールから繰り出した一次連続シートを重ね合わせて巻き取るとともに輪切り(幅方向に複数に分割)にし、複数枚のプライからなる二次原反ロールを製造する。
<Manufacturing form>
First, the manufacturing method according to the present invention will be described.
In the production of the box-type tissue paper, after making thin paper from pulp fibers (preferably 100% virgin pulp fiber not containing waste paper pulp) in a paper machine, crepe if necessary, calendering, This is wound up to produce a primary raw roll (generally referred to as a jumbo roll), and although not shown, this primary raw roll is set in a known ply machine, and is delivered from a plurality of primary raw rolls. The continuous sheet is overlapped and wound, and is cut into a plurality of pieces (divided into a plurality in the width direction) to produce a secondary raw roll made of a plurality of plies.

プライマシンで製造した二次原反ロールは、プライマシンから取り出されその後図1に示すインターフォルダにセットされる。インターフォルダにおいては、二次原反ロールから繰り出した二次連続シートを折り畳みながら積み重ねる。インターフォルダで製造した折り畳み積層物は、後段設備において長手方向に所定の間隔をおいて裁断され、箱詰め、包装等の処理を経て製品となる。   The secondary web roll produced by the ply machine is taken out from the ply machine and then set in the interfolder shown in FIG. In the inter folder, the secondary continuous sheets fed out from the secondary material roll are stacked while being folded. The folded laminate manufactured by the interfolder is cut at a predetermined interval in the longitudinal direction in the subsequent equipment, and becomes a product through processing such as boxing and packaging.

図1は、本発明におけるインターフォルダでの工程を示している。
すなわち、インターフォルダにおいて、パルプ繊維を抄造した原紙を、所定の幅(通常は、製品幅もしくはその複数倍の幅とされる)で巻き取った前記の二次原反ロールとしての巻取ロール1、2から連続シート10、20をそれぞれ巻き戻して、これらを折り畳み積み重ね手段50により折り畳み積み重ねるのである。
FIG. 1 shows a process in an interfolder according to the present invention.
That is, in the inter folder, the winding roll 1 as the above-mentioned secondary raw roll obtained by winding a base paper made of pulp fibers with a predetermined width (usually a product width or a multiple of the width). 2, the continuous sheets 10 and 20 are rewound, and are folded and stacked by the folding and stacking means 50.

図示のインターフォルダの組は、図面を貫く方向に多数有し、最終的な折り畳み積層物は、後段設備において長手方向に製品幅と等しい間隔をおいて裁断され、箱詰め、包装等の処理を経て製品されるのである。   The set of interfolders shown in the figure has a large number in the direction penetrating the drawing, and the final folded laminate is cut at intervals equal to the product width in the longitudinal direction in the subsequent equipment, and subjected to processing such as boxing and packaging. It is manufactured.

さて、巻取ロール1、2からそれぞれ2プライの連続シート10、20は、テンションコントローラ31、41にて張力制御がなされた後、細幅のエンボスロールを有しこれと弾性ロールとの間でシートを押圧状態でニップするプライ接合手段32、42にてプライ接合される。その後、薬液パンを有し、その薬液をグラビアロールにピックアップして、対象のシートに薬液を転写するロール転写装置33,34及び43、44により薬液をロール転写で連続的に塗布する。ここで、2プライの連続シート10及び20に対し、2つのロール転写装置33,34及びロール転写装置43,44を備えているのは、連続シート10及び20がそれぞれ2プライであり、各外面に薬液を塗布するためである。   Now, the two-ply continuous sheets 10 and 20 from the take-up rolls 1 and 2 are subjected to tension control by the tension controllers 31 and 41, and then have a narrow embossing roll between this and the elastic roll. Ply bonding is performed by ply bonding means 32 and 42 that nip the sheet in a pressed state. Thereafter, a chemical liquid pan is provided, the chemical liquid is picked up by a gravure roll, and the chemical liquid is continuously applied by roll transfer by roll transfer devices 33, 34, 43, and 44 that transfer the chemical liquid to a target sheet. Here, the two-ply continuous sheets 10 and 20 are provided with the two roll transfer devices 33 and 34 and the roll transfer devices 43 and 44, respectively. This is because a chemical solution is applied to the skin.

このように薬液を塗布した後、プレス装置35、45により薬液を含浸させる工程を取り入れるのが望ましい。プレス装置35、45を使用することで、薬液の含浸を図ることができるばかりでなく、幅方向の含浸量の均一化を図ることもできる。   After applying the chemical solution in this way, it is desirable to incorporate a step of impregnating the chemical solution with the press devices 35 and 45. By using the press devices 35 and 45, not only can the chemical solution be impregnated, but also the amount of impregnation in the width direction can be made uniform.

その後は、前述のように、連続シート10及び20は折り畳み積み重ね手段50により折り畳み積み重ねられる。   Thereafter, the continuous sheets 10 and 20 are folded and stacked by the folding and stacking means 50 as described above.

ここでプライボンディングについて説明する。この種のティッシュペーパーはエンボス加工によりプライ(薄葉紙層)相互が接合され、使用に際して離れないようになっている。このためプライマシンとインターフォルダとを個別に備えた設備では、従来においては、プライマシンにおいて一次連続シート相互を重ね合わせてから巻き取りまでの間に、エンボスロールによってエンボス接合を行っていた。プライマシンにおける処理速度はインターフォルダと比べて速いため、ここでエンボス接合加工を施すと、エンボスを均一に付与できずにプライ離れが生じ易くなったり、エンボス付与部における紙の裂けや断紙が発生し易くなったり、プライボンディング(重ね合わせ接合)が不安定になったりするという問題点があった。   Here, ply bonding will be described. In this type of tissue paper, the plies (thin paper layers) are joined to each other by embossing so that they do not leave in use. For this reason, in the equipment provided with the ply machine and the interfolder individually, conventionally, the embossing is performed by the embossing roll between the primary continuous sheets in the ply machine and the winding. Since the processing speed of the ply machine is faster than that of the interfolder, if emboss bonding is applied here, embossing cannot be uniformly applied and ply separation is likely to occur, or paper tearing or breakage at the embossing portion may occur. There is a problem that it tends to occur and ply bonding (overlap bonding) becomes unstable.

そこで、本出願人が特開2002―347146号に開示したように、エンボス加工による接合が行われていないそれぞれ複数枚のプライからなる複数の連続シートを、インターフォルダに供給し、前記連続シートの折り畳み積み重ねに先立って、前記連続シートにエンボス加工を施しプライ相互を接合することが望ましい。   Therefore, as disclosed in JP-A-2002-347146, the present applicant supplies a plurality of continuous sheets each composed of a plurality of plies that are not joined by embossing to an interfolder, Prior to folding and stacking, it is desirable to emboss the continuous sheet to join the plies together.

この場合、図1に示すように、プライ接合手段32、42をロール転写装置33,34及び43、44より前段に配設することが望ましい。逆であると、薬液塗布がシートの全面であり、そのシート幅の両側にプライボンディングを行うときに、その接合強度が低下するからである。   In this case, as shown in FIG. 1, it is desirable to arrange the ply joining means 32 and 42 in front of the roll transfer devices 33, 34 and 43, 44. If the reverse is true, the chemical solution is applied to the entire surface of the sheet, and the bonding strength decreases when ply bonding is performed on both sides of the sheet width.

ここで、原紙の抄造工程において、本発明の対象薬液以外の別種の薬液、たとえば界面活性剤からなる柔軟剤、でんぷんやデキストリンなどの湿潤紙力剤、カルボキシメチルセルロースなどの一種または二種以上を塗布すると、本発明の対象薬液と相俟って風合いを改善できる。   Here, in the base paper making process, another kind of chemical solution other than the target chemical solution of the present invention, for example, a softening agent comprising a surfactant, a wet paper strength agent such as starch or dextrin, or one or more of carboxymethyl cellulose is applied. Then, the texture can be improved in combination with the target drug solution of the present invention.

<薬液等>
いわゆるローション薬液の塗布にあたり、抄造後の約6%程度の水分率を示すシート単位容積当たりの含有量を12〜45mg/cm3、特に18〜40mg/cm3とするのが望ましい。薬液含有量が少ないと次記の目的特性を得がたい。薬液含有量を多くすると、薬液使用量の増大に伴いコスト高となるばかりでなく、使用時におけるベトツキ感及び使用後における薬液の残存感を与える。本発明において、少ない薬液使用量にもかかわらず、次記の目的特性を与えるのは米坪を低くすることとの関係が大きい。
<Chemicals>
In applying the so-called lotion chemical solution, it is desirable that the content per sheet unit volume showing a moisture content of about 6% after paper making is 12 to 45 mg / cm 3 , particularly 18 to 40 mg / cm 3 . If the chemical content is low, it is difficult to obtain the following target characteristics. Increasing the chemical solution content not only increases the cost as the chemical solution is used, but also gives a feeling of stickiness during use and a residual feeling of the chemical solution after use. In the present invention, in spite of a small amount of the chemical solution used, the following characteristics are largely related to lowering the rice paper weight.

すなわち、本発明の原紙の望ましい1プライ当たりの米坪は10〜25g/m2、特に好ましくは10〜15g/m2である。米坪が低いことにより紙のコシを弱くすることができ、充分に柔軟性に富むものとなる。ただし、過度に低いと強度の低下などを生じる。 That is, the desirable rice basis weight per ply of the base paper of the present invention is 10 to 25 g / m 2 , particularly preferably 10 to 15 g / m 2 . Since the rice tsubo is low, the stiffness of the paper can be weakened, and it becomes sufficiently flexible. However, if it is too low, the strength will decrease.

製品のソフトネスは0.5〜1.0g、特に0.6〜0.8であるのが望ましい。   The softness of the product is preferably 0.5 to 1.0 g, particularly 0.6 to 0.8.

本発明におけるローション薬液に限定されるものではないが、主に、肌触り性(風合い)を高めたり、保湿性を高め、パルプ繊維の肌への刺激を和らげるあるいは潤い感を高めることを主眼とするものを挙げることができる。   Although it is not limited to the lotion chemical | medical solution in this invention, it mainly focuses on improving the touch (texture), moisturizing property, reducing the irritation | stimulation to the skin of a pulp fiber, or raising a moist feeling. Things can be mentioned.

たとえば、保湿性薬液として、シリコーンオイル、シリコーンパウダー等のポリシロキサン、グリセリン、ジグリセリン、プロピレングリコール、1,3−ブチレングリコール、ポリエチレングリコール等の多価アルコール、ソルビトール、グルコース、キシリトール、マルトース、マルチトール、マンニトール、トレハロース等の糖類、グリコール系溶剤およびその誘導体のうちの少なくとも1種の保湿剤を含むものを用いてなるものを挙げることができる。
さらに、セタノール、ステアリルアルコール、オレイルアルコール等の高級アルコール、流動パラフィンなども使用できる。
Examples of moisturizing chemicals include polysiloxanes such as silicone oil and silicone powder, polyhydric alcohols such as glycerin, diglycerin, propylene glycol, 1,3-butylene glycol, and polyethylene glycol, sorbitol, glucose, xylitol, maltose, and maltitol. And saccharides such as mannitol and trehalose, glycol solvents, and derivatives containing at least one moisturizing agent among derivatives thereof.
Furthermore, higher alcohols such as cetanol, stearyl alcohol and oleyl alcohol, liquid paraffin and the like can be used.

また、前記薬液に、グリシン、アスパラギン酸、アルギニン、アラニン、シスチン、システインなどのアミノ酸;アロエエキス、アマチャエキス、カリンエキス、キュウリエキス、アギナエキス、トマトエキス、ノバラエキス、ヘチマエキス、ユリエキス、レンゲソウエキスなどの植物抽出エキス;オリーブ油、ホホバ油、ローズヒップ油、アーモンド油、ユーカリ油、アボガド油、ツバキ油、大豆油、サフラワー油、ゴマ油、月見草油などの植物油;ビタミン、加水分解コラーゲン、加水分解ケラチン、加水分解シルク、キトサン、尿素、はちみつ、ローヤルゼリー、ヒアルロン酸ナトリウム、セラミド、スクワラン、ワセリンなどを配合できる。
ここで、ビタミンC、ビタミンE、コラーゲンがある。この種のものは、潤い感を高め機能がある。ビタミンCおよびビタミンEは抗酸化剤としても機能する。ビタミンEは還元力の強い成分で、活性酸素・フリーラジカルを消去したり過酸化脂質の発生を防ぐ抗酸化作用がある。よってビタミンEは薬液の安定化剤として機能するとともに、薄葉紙を使用した者の肌に付与されると当該肌の皮脂の酸化防止効果および血行促進効果が発揮される。また保湿機能もある。ビタミンCはビタミンEと同じく皮脂の抗酸化作用がある。またビタミンCはビタミンEを還元する作用があるため、ビタミンC,Eの両方を用いると、ビタミンCがビタミンEの助剤として働き、活性酸素などにより酸化されたビタミンEを還元し、ビタミンEの強力な皮脂の抗酸化作用を維持する作用が奏せられる。コラーゲンは肌の真皮の90%を形成しており、これが減少すると肌に潤いや張りがなくなる。よって、薄葉紙に含有させておくことによって、これが肌と接触したときに肌に潤いを与える保湿効果を発揮するとともに、薄葉紙に対しても保湿効果を発揮する。
In addition, in the chemical solution, amino acids such as glycine, aspartic acid, arginine, alanine, cystine, cysteine; Plant extract: olive oil, jojoba oil, rosehip oil, almond oil, eucalyptus oil, avocado oil, camellia oil, soybean oil, safflower oil, sesame oil, evening primrose oil, etc .; vitamins, hydrolyzed collagen, hydrolyzed keratin, Hydrolyzed silk, chitosan, urea, honey, royal jelly, sodium hyaluronate, ceramide, squalane, petrolatum and the like can be blended.
Here, there are vitamin C, vitamin E, and collagen. This type has a moisturizing function. Vitamin C and vitamin E also function as antioxidants. Vitamin E is a component with a strong reducing power and has an antioxidative action that eliminates active oxygen and free radicals and prevents the generation of lipid peroxide. Therefore, vitamin E functions as a chemical liquid stabilizer, and when applied to the skin of a person who uses thin paper, the effect of preventing the sebum of the skin and promoting blood circulation are exhibited. There is also a moisturizing function. Vitamin C, like vitamin E, has sebum antioxidant activity. Vitamin C has the action of reducing vitamin E, so if both vitamin C and E are used, vitamin C works as an auxiliary to vitamin E, reducing vitamin E oxidized by active oxygen, etc. The effect of maintaining the strong anti-oxidant effect of sebum is exhibited. Collagen forms 90% of the dermis of the skin, and when this decreases, the skin loses moisture and tension. Therefore, by making it contain in thin paper, while exhibiting the moisturizing effect which moisturizes skin when this contacts with skin, the moisturizing effect is exhibited also to thin paper.

さらに、薬液としては、特にpHが5.0〜6.0の弱酸性とされたものであると、肌に対して接触させても肌がアルカリ性になることがなく、薬液pHの影響による肌荒れを効果的に防止できる。特に好適なpH範囲は5.3〜5.7である。pHの調整法としては、酸性または塩基性のpH調整剤を薬液に添加することにより行うことができ、薬液が強酸性の場合には水酸化ナトリウム水溶液や水酸化カリウム水溶液を用いることができ、中性・アルカリ性の場合にはクエン酸やリンゴ酸、乳酸を用いることができる。   Furthermore, as a chemical solution, when the pH is set to be weakly acidic with a pH of 5.0 to 6.0, the skin does not become alkaline even when brought into contact with the skin, and the skin is rough due to the influence of the chemical solution pH. Can be effectively prevented. A particularly preferred pH range is 5.3 to 5.7. The pH can be adjusted by adding an acidic or basic pH adjuster to the chemical solution. When the chemical solution is strongly acidic, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution can be used. In the case of neutral / alkaline, citric acid, malic acid and lactic acid can be used.

清涼感を得るための薬液として、ソルビトール、アルチトール、キシリトール、エリスリトール、ラクチトール、パラチニットを挙げることができる。特に好ましいものは、エリスリトール、キシリトール、ソルビトールであり、さらに好ましくはエリスリトール又はキシリトールである。さらに、メントール、サリチル酸、α−シネロール、及びこれらの誘導体の群から選ばれた一種又は二種以上の冷感剤を含ませることができる。この場合、上記清涼感を得るための薬剤をバインダー成分中に分散された状態で紙基材表面に偏在して含ませるのが望ましい。   Examples of the chemical solution for obtaining a refreshing sensation include sorbitol, altitol, xylitol, erythritol, lactitol, and palatinit. Particularly preferred are erythritol, xylitol and sorbitol, and more preferred is erythritol or xylitol. Furthermore, one or two or more kinds of cooling sensitizers selected from the group of menthol, salicylic acid, α-cinerol, and derivatives thereof can be included. In this case, it is desirable that the agent for obtaining the refreshing feeling is contained unevenly on the surface of the paper base material in a state dispersed in the binder component.

一方、原紙の抄造段階で添加することが望ましい添加剤としては、湿潤紙力剤、柔軟剤及びカルボキシメチルセルロースなどである。   On the other hand, additives desirable to be added in the papermaking stage include wet paper strength agents, softeners and carboxymethylcellulose.

柔軟剤の代表例は、界面活性剤系の柔軟剤であり、その柔軟剤としては、アニオン系界面活性剤、非イオン系界面活性剤、カチオン系界面活性剤および両性イオン界面活性剤のなかから適宜選択して用いることができる。アニオン系界面活性剤を用いた場合、基材紙のコシ(曲げ剛性)を前述の範囲まで低下させることができ、もって保湿剤による潤い感や柔軟剤による柔らか感を助長することができる。アニオン系界面活性剤としては、カルボン酸塩系、スルホン酸塩系、硫酸エステル塩系、燐酸エステル塩系などを用いることができる。特にアルキル燐酸エステル塩が好ましい。   A typical example of a softener is a surfactant-based softener, and examples of the softener include anionic surfactants, nonionic surfactants, cationic surfactants, and zwitterionic surfactants. It can be appropriately selected and used. When an anionic surfactant is used, the stiffness (bending rigidity) of the base paper can be reduced to the above-described range, and thus the moisturizing feeling by the moisturizing agent and the soft feeling by the softening agent can be promoted. As the anionic surfactant, carboxylate, sulfonate, sulfate ester, phosphate ester, and the like can be used. An alkyl phosphate ester salt is particularly preferable.

非イオン界面活性剤としては、ソルビタン脂肪酸エステル、ジエチレングリコールモノステアレート、ジエチレングリコールモノオレエート、グリセリルモノステアレート、グリセリルモノオレート、プロピレングリコールモノステアレートなどの多価アルコールモノ脂肪酸エステル、N−(3−オレイロシキ−2−ヒドロキシプロピル)ジエタノールアミン、ポリオキシエチレン硬化ヒマシ油、ポリオキシエチレンソルビット密ロウ、ポリオキシエチレンソルビタンセスキステアレート、ポリオキシエチレンモノオレエート、ポリオキシエチレンモノラウレート、ポリオキシエチレンセチルエーテル、ポリオキシエチレンラウリルエーテルなどを用いることができる。   Examples of nonionic surfactants include sorbitan fatty acid esters, diethylene glycol monostearate, diethylene glycol monooleate, glyceryl monostearate, glyceryl monooleate, and polyhydric alcohol monofatty acid esters such as N- (3- Oleiroshiki-2-hydroxypropyl) diethanolamine, polyoxyethylene hydrogenated castor oil, polyoxyethylene sorbitan beeswax, polyoxyethylene sorbitan sesquistearate, polyoxyethylene monooleate, polyoxyethylene monolaurate, polyoxyethylene cetyl ether Polyoxyethylene lauryl ether can be used.

本発明の柔軟剤としては、カチオン界面活性剤を使用するのが望ましい。このカチオン界面活性剤としては、第4級アンモニウム塩、アミン塩、またはアミンなどをもちいることができる。また、両性イオン界面活性剤としては、カルボキシ、スルホネート、サルフェートを含有する第2級または第3級アミンの脂肪族誘導体、または複素環式第2級または第3級アミンの脂肪族誘導体などを用いることができる。   As the softener of the present invention, it is desirable to use a cationic surfactant. As the cationic surfactant, a quaternary ammonium salt, an amine salt, an amine, or the like can be used. In addition, as the zwitterionic surfactant, an aliphatic derivative of a secondary or tertiary amine containing carboxy, sulfonate, sulfate, an aliphatic derivative of a heterocyclic secondary or tertiary amine, or the like is used. be able to.

湿潤紙力(増強)剤としては、メラミン−ホルムアルデヒド付加縮合物、尿素−ホルムアルデヒド付加縮合物のほか、環境を考慮すると、次述するものが好適に使用できる。ポリアクリルアミド、ポリビニルアルコール、グリオキザール・ポリアクリルアミド共重合物、官能基数を通常の1/10に低減したポリアミドエピクロルヒドリン樹脂、ジアルデヒドスターチまたはカチオン変性デンプン、酸化デンプン等、より具体的にはカチオン性を有するポリビニルアミド共重合体と二価アルデヒドからなる熱硬化性樹脂(例えば、特公昭44−26670号公報、特公昭54−44762号公報、特開昭57−149595号公報)、カチオン性アルデヒド変性ポリアクリルアミド共重合体(特開平6−184985号公報、特開平8−56868号公報)、カチオン性高分子とアニオン性高分子を含有し、カチオン性高分子及びアニオン性高分子の少なくとも1つの高分子が疎水性を有するもの(特開2002−275787号公報)等、公知のものを用いることができる。   As the wet strength (enhancement) agent, in addition to the melamine-formaldehyde addition condensate and the urea-formaldehyde addition condensate, the following can be preferably used in consideration of the environment. Polyacrylamide, polyvinyl alcohol, glyoxal / polyacrylamide copolymer, polyamide epichlorohydrin resin whose number of functional groups is reduced to 1/10 of the usual number, dialdehyde starch or cation-modified starch, oxidized starch, etc. More specifically, it has a cationic property. Thermosetting resins comprising a polyvinylamide copolymer and a divalent aldehyde (for example, Japanese Patent Publication No. 44-26670, Japanese Patent Publication No. 54-44762, Japanese Patent Publication No. 57-149595), cationic aldehyde-modified polyacrylamide A copolymer (JP-A-6-184985, JP-A-8-56868), a cationic polymer and an anionic polymer, wherein at least one polymer of the cationic polymer and the anionic polymer is Hydrophobic (JP 2002-2002 75787 JP) or the like, it can be used known ones.

<添加剤配合>
本発明の好適な添加剤配合を下記に示す。
・有効成分 60〜100重量%(特に80〜100重量%)
薬液 95.5〜97.0重量%
柔軟剤、湿潤紙力剤及びCMCの少なくとも一種 3.0〜4.5重量%
・水分 0〜40重量%
<Additive formulation>
A preferred additive formulation of the present invention is shown below.
Active ingredient 60-100% by weight (especially 80-100% by weight)
Chemical solution 95.5-97.0% by weight
At least one kind of softener, wet paper strength agent and CMC 3.0 to 4.5% by weight
・ Moisture 0-40% by weight

<製造条件等>
本発明の衛生薄葉紙を製造するにあたっては、抄紙工程では望ましくは1プライ当たりの10〜25g/m2、最適には10〜15g/m2での範囲となるように原料パルプおよび抄紙条件を調整する。原料パルプとしては、必要により50%以下の割合で古紙パルプを含ませることもできるが、バージンパルプであるのが望ましく、NBKP及びLBKPから構成され、NBKPの割合が30〜70%、特に40〜60%が望ましい。そして、湿潤紙力剤、柔軟剤及びカルボキシメチルセルロース(CMC)を添加し、抄造するのが望ましい。
<Manufacturing conditions>
In the production of the sanitary thin paper of the present invention, the raw pulp and papermaking conditions are adjusted so that the range of 10-25 g / m 2 per ply is optimal and 10-15 g / m 2 is optimal in the paper making process. To do. As a raw material pulp, waste paper pulp can be included at a ratio of 50% or less as necessary, but is preferably virgin pulp, and is composed of NBKP and LBKP, and the ratio of NBKP is 30 to 70%, particularly 40 to 40%. 60% is desirable. Then, it is desirable to add a wet paper strength agent, a softening agent, and carboxymethyl cellulose (CMC) to make paper.

このとき原料パルプの叩解幅を狭めて高密度化することができる。一般的には米坪を規定して高密度化すると、紙力が高まり紙厚が低下しふんわり感は出なくなるが、後のクレープ処理工程において、クレープの刃先角度を調整して、クレープ率を高めるようにするとふんわり感がでるようになる。   At this time, the beating width of the raw pulp can be narrowed to increase the density. In general, when the density is increased by specifying the rice tsubo, the paper strength increases and the paper thickness decreases and the soft feeling does not appear.However, in the subsequent creping process, the crepe blade angle is adjusted to increase the crepe rate. If you increase it, you will feel soft.

そして、最終的にカレンダー処理工程において、紙厚が過度に低下して目的の紙厚の範囲から外れないようにオンラインマシンカレンダーおよびプライマシンカレンダーの各カレンダー処理における圧力を調整してカレンダー処理する。   Finally, in the calendar processing step, the calendar processing is performed by adjusting the pressure in each calendar processing of the online machine calendar and the ply machine calendar so that the paper thickness does not fall excessively and falls outside the range of the target paper thickness.

すなわち、上記の製造方法をとると、原料パルプの叩解幅を狭めて高密度化により紙厚が薄くかつ表面の平滑度の高い原紙が形成され、その原紙に対して高いクレープ率でクレープ加工することにより滑らかさを有しつつふっくらとした感じが発現し、その後のカレンダー処理において、最終的な紙厚が調整される。なお、具体的な、クレープ率や、使用する製造設備、添加剤、原料パルプの配合割合により適宜調整すればよい。   That is, when the above production method is adopted, a raw paper having a thin paper thickness and a high surface smoothness is formed by narrowing the beating width of the raw pulp and increasing the density, and the raw paper is creped at a high crepe rate. As a result, a fluffy feeling is developed while having smoothness, and the final paper thickness is adjusted in the subsequent calendar processing. In addition, what is necessary is just to adjust suitably with the specific crepe rate, the manufacturing equipment to be used, an additive, and the mixture ratio of raw material pulp.

本発明の家庭用衛生薄葉紙の1プライ当たりの米坪は、前述のように、10〜25g/m2の2プライ製品が望ましいが、必要ならば、3プライ以上に積層できる。 As described above, the two-ply product of 10 to 25 g / m 2 is desirable as the rice basis weight per ply of the household sanitary thin paper of the present invention.

<オイルKES肌触り指数>
オイルKES肌触り指数は6.5以下であるのが望ましい。
この測定には、通常のMMD試験機、例えば、図2〜図4に示すように、カトーテック株式会社製の摩擦感テスター「KES SE」の基台上に人工皮革(サプラーレ:出光テクノファイン社製)を敷いて固定するとともに、測定端子Tを人工皮革(サプラーレ:出光テクノファイン社製)にて被覆し、その測定端子の測定面の人工皮革で被覆された部分(接触平面)にオリーブオイル(BOSCOエクストラバージンオイル:日清精油)4mgを均一に塗布し、MMDの測定手順と同様にして行なうことができる。詳細には、人工皮革で構成される接触平面は、横断面直径0.5mmにピアノ線からなり、先端の曲率半径が0.25mmの単位膨出部が隣接して有し、全幅が10mmの連続した測定面を有し、その測定面の長さが10mmとされるほぼ10mm四方の測定面を有するMMD測定用端子を、前記人工皮革で被覆して形成することができる。人工皮革による前記端子の被覆は、10mm四方の接触平面が形成されるように端子の測定面に対して人工皮革がぴったりと接触するように、あるいは若干の張力をもたせてぴったりと被覆することにより達成できる。人工皮革を端子に固定するにあたっては、測定時、すなわち紙試料を移動させたときに人工皮革と内部の端子とがずれて人工皮革に接触平面に歪みなどが生じないようにしっかりと固定することが重要である。固定は例えば、前記接触平面が構成されるように前記端子を被覆したのち、接触平面を構成しない部位を輪ゴム等で装置の測定に影響が出ない部位、例えば端子の支持材等にしっかり固定する。また、MMD試験機の基台上には人工皮革を敷いて接着テープ等で固定する。このとき、測定時に歪まないように基台に人工皮革をしっかりと固定することが重要である。また、基台上に敷く人工皮革は、前記接触平面を構成する人工皮革と同じものを用いる。なお、紙試料は、10cm四方に裁断して用い、人工皮革を敷いた基台に固定する。測定に際しては、紙試料の上に試料押さえ用錘(約100g)で押さえる。また、試験機の測定端子への荷重を50gとして人工皮革で構成される接触平面全体が50gf/cm2の接触圧で紙試料に接触するようにするが、これは、MMD測定と同様に、円盤状の錘を端子上部に取り付けることで達成できる。もちろん、支持材の一方の端部(紙試料の移動方向と反対の端部)の固定の仕方はMMDの測定に準ずる。測定は、紙試料の縦方向について3回、横方向について3回の計6回を行い、測定値についてはその6回の平均値とする。
<Oil KES touch index>
The oil KES touch index is preferably 6.5 or less.
For this measurement, as shown in FIGS. 2 to 4, an artificial leather (supplera: Idemitsu Techno Fine Co., Ltd.) is placed on the base of a friction tester “KES SE” manufactured by Kato Tech Co., Ltd. The measuring terminal T is covered with artificial leather (supplera: manufactured by Idemitsu Techno Fine Co., Ltd.), and olive oil is applied to the measuring surface of the measuring terminal covered with artificial leather (contact plane). (BOSCO extra virgin oil: NISSIN SEIMITSU OIL) 4 mg can be uniformly applied, and the measurement can be performed in the same manner as the MMD measurement procedure. Specifically, the contact plane made of artificial leather is composed of a piano wire with a cross-sectional diameter of 0.5 mm, adjacent to a unit bulging portion with a radius of curvature of 0.25 mm at the tip, and a total width of 10 mm. An MMD measurement terminal having a continuous measurement surface and a measurement surface of approximately 10 mm square with a measurement surface length of 10 mm can be formed by covering with the artificial leather. The covering of the terminal with the artificial leather is carried out by covering the terminal with the artificial leather so that a contact plane of 10 mm square is formed or so that the artificial leather is in close contact with the measurement surface of the terminal or with a slight tension. Can be achieved. When fixing the artificial leather to the terminal, make sure to fix the artificial leather so that the artificial leather and the internal terminal do not move and the contact plane is distorted during measurement, that is, when the paper sample is moved. is important. For example, after the terminal is covered so that the contact plane is formed, a portion that does not form the contact plane is firmly fixed to a portion that does not affect the measurement of the apparatus with a rubber band or the like, for example, a support material of the terminal. . Also, artificial leather is laid on the base of the MMD testing machine and fixed with adhesive tape or the like. At this time, it is important to firmly fix the artificial leather to the base so as not to be distorted during measurement. The artificial leather laid on the base is the same as the artificial leather constituting the contact plane. In addition, the paper sample is cut into a 10 cm square and used, and is fixed to a base on which artificial leather is laid. At the time of measurement, a sample pressing weight (about 100 g) is pressed on a paper sample. In addition, the load on the measuring terminal of the testing machine is set to 50 g, and the entire contact plane made of artificial leather is brought into contact with the paper sample with a contact pressure of 50 gf / cm 2. This is similar to the MMD measurement. This can be achieved by attaching a disk-shaped weight to the top of the terminal. Of course, the method of fixing one end of the support material (the end opposite to the moving direction of the paper sample) conforms to the MMD measurement. The measurement is performed three times in the vertical direction of the paper sample and three times in the horizontal direction, for a total of 6 times, and the measured value is the average of the 6 times.

NBKP60%、LBKP40%配合のパルプをフリーネス約600ml(CSF)に叩解して、原紙米坪14.0g/m2、クレープ率((製紙時のドライヤーの周速)−(リール周速))/(製紙時のドライヤーの周速)×100)が21%の衛生紙用原紙を抄紙し、家庭用衛生薄葉紙の形状(2枚重ね、縦211mm、横231.5mm)に加工した。
この場合、米坪及び薬液の塗布形態を代えて各特性を調べた。結果を表1に示す。
A pulp containing 60% NBKP and 40% LBKP is beaten to a freeness of about 600 ml (CSF), and the base paper is 14.0 g / m 2 , crepe rate ((peripheral speed of the dryer during papermaking)-(reel peripheral speed)) / The base paper for sanitary paper having a (peripheral speed of the dryer at the time of paper making) × 100) of 21% was made and processed into a sanitary thin paper for home use (two stacked, 211 mm long, 231.5 mm wide).
In this case, each characteristic was investigated by changing the coating form of the rice tsubo and the chemical solution. The results are shown in Table 1.

実施例1は、図1に示し前述の製造方法による例である。従来例1は、本出願人が特開2003―164385号の提案過程で実験した例である。すなわち、前述の薬液をインターフォルダにかける前にオフラインでロール塗工したものである。比較例1〜比較例3は現在の市販品であり、薬液塗布方式の欄の記載は、予想に基づくものである。   Example 1 is an example of the manufacturing method shown in FIG. Conventional example 1 is an example in which the present applicant experimented in the proposing process of Japanese Patent Laid-Open No. 2003-164385. That is, the above-described chemical solution is roll-coated offline before being applied to the interfolder. Comparative Examples 1 to 3 are currently commercially available products, and the descriptions in the column of the chemical solution application method are based on expectations.

なお、測定条件は次記のとおりである。
(1) 米坪(1プライ)の測定:JIS P 8214
(2) 紙厚(2プライ)の測定:紙厚は、JIS P 8111の条件下で、尾崎製作所ダイヤルシックネスゲージ「PEACOCK G型」を用いて測定する。具体的には、プランジャーと測定台の間にゴミ、チリ等がないことを確認してプランジャーを測定台の上におろし、前記ダイヤルシックネスゲージのメモリを移動させてゼロ点を合わせ、次いで、プランジャーを上げて試料(ティシュペーパー)を試験台の上におき、プランジャーをゆっくりと下ろしそのときのゲージを読み取る。このとき、プランジャーをのせるだけとする。なお、測定は1枚で行い、10回の平均値とする。
(3) 薬液含有量:ソックスレー抽出器により、試料約10gを、エタノール・ベンゼン溶剤(容積比1:1)120〜140mlによる温浴上で抽出液が軽く沸騰を保つ程度に4時間加熱し抽出する。その後、150±2℃の恒温乾燥器中に90分放置し、抽出分の重量を測定し、試料の絶乾燥重量により除してその比率を%で求める。
(4) 紙の単位容積当たりの薬液含有量:薬液含有量=米坪(1プライ当り)×2(プライ)×薬液含有量(%)×1000÷(単位面積当りの容積)
ただし、単位面積当りの容積は紙厚(μm)÷10000×100×100である。
(5) 水分率:前掲
(6) ソフトネス:ハンドルオメーター
(7) オイルKES肌触り指数:前掲
(8) MMD:表面特性試験機(カトーテック社製「摩擦感テスター KESSE」)。
The measurement conditions are as follows.
(1) Measurement of US tsubo (1 ply): JIS P 8214
(2) Measurement of paper thickness (2-ply): The paper thickness is measured using an Ozaki Dial Thickness Gauge “PEACOCK G type” under the conditions of JIS P8111. Specifically, confirm that there is no dust, dust, etc. between the plunger and the measuring table, lower the plunger on the measuring table, move the memory of the dial thickness gauge to adjust the zero point, and then Then, raise the plunger and place the sample (tissue paper) on the test table, slowly lower the plunger and read the gauge at that time. At this time, only the plunger is placed. In addition, a measurement is performed by 1 sheet and it is set as the average value of 10 times.
(3) Chemical solution content: About 10 g of sample is extracted with a Soxhlet extractor by heating for 4 hours to keep the extract lightly boiling on a warm bath with 120-140 ml of ethanol / benzene solvent (volume ratio 1: 1). . Thereafter, the sample is left in a constant temperature dryer at 150 ± 2 ° C. for 90 minutes, the weight of the extract is measured, and the ratio is determined by dividing by the dry weight of the sample.
(4) Chemical solution content per unit volume of paper: Chemical solution content = US tsubo (per ply) x 2 (ply) x chemical solution content (%) x 1000 ÷ (volume per unit area)
However, the volume per unit area is paper thickness (μm) ÷ 10000 × 100 × 100.
(5) Moisture content: supra
(6) Softness: Handle ohmmeter
(7) Oil KES feel index: supra
(8) MMD: Surface property testing machine (“Friction Tester KESSE” manufactured by Kato Tech).

Figure 2012030125
Figure 2012030125

実施例1は、インターフォルダにおいて、巻き戻しから折り畳み積み重ね工程の間で、連続シートにいわゆるローション薬液をロール転写で連続的に塗布するものである。表1の結果から判るように、ロール転写により薬液を塗布すると、スプレー塗布による場合より、基材紙への薬液の塗布量を多くすることができる。また、インターフォルダにおいてオンライン塗布を行うので、紙の伸びを生じることがなく、米坪を低いものとすることができ、紙のコシが小さいあるいは風合いに優れたものとすることができ、もって、少ない薬液塗布量であっても柔軟性に富むものを得ることができる。この米坪を低く、薬液塗布量を少なくすることは経済性に優れることを意味する。   In the first embodiment, in the interfolder, a so-called lotion chemical solution is continuously applied to a continuous sheet by roll transfer between unwinding and folding and stacking steps. As can be seen from the results in Table 1, when the chemical solution is applied by roll transfer, the amount of the chemical solution applied to the base paper can be increased as compared with the case of spray coating. In addition, since the online application is performed in the interfolder, the paper does not stretch, the basis weight of the paper can be lowered, the paper is less stiff or has an excellent texture, Even with a small amount of chemical solution applied, a product with high flexibility can be obtained. Lowering the rice tsubo and reducing the amount of the chemical solution applied means better economy.

本発明の家庭用衛生薄葉紙の製造形態の概要図である。It is a schematic diagram of the manufacture form of the household sanitary thin paper of this invention. オイルKES肌触り指数の測定端子および測定時の概略を示す図である。It is a figure which shows the measurement terminal of the oil KES touch index, and the outline at the time of a measurement. 表面特性の測定装置の例の概略を示す図である。It is a figure which shows the outline of the example of the measuring apparatus of surface characteristics. その接触平面の構成を説明するための図である。It is a figure for demonstrating the structure of the contact plane.

2…巻取ロール、10、20…連続シート、50…折り畳み積み重ね手段、32、42…プライ接合手段、33,34、43、44…ロール転写装置、35、45…プレス装置。   DESCRIPTION OF SYMBOLS 2 ... Winding roll, 10, 20 ... Continuous sheet, 50 ... Folding and stacking means, 32, 42 ... Ply joining means, 33, 34, 43, 44 ... Roll transfer device, 35, 45 ... Press device.

Claims (2)

インターフォルダにおいて、パルプ繊維を抄造した原紙を所定の幅で巻き取った巻取ロールから連続シートをそれぞれ巻き戻して、これらを折り畳み積み重ねて製品化する家庭用衛生薄葉紙の製造方法において、
抄造工程で前記原紙に対して、有効成分として、湿潤紙力剤、柔軟剤およびカルボキシメチルセルロースの少なくとも一種を添加剤として予め添加しておき、
前記インターフォルダにおける巻き戻しから折り畳み積み重ね工程の間で、前記連続シートに、有効成分として前記添加剤とは別の保湿性薬液をpHを5.0〜6.0に調整してグラビアロールによるロール転写で連続的に塗布し、その後にプレス装置により前記薬液を含浸させて、シート単位容積当たりの薬液含有量を12〜45mg/cm3とする、ことを特徴とする家庭用衛生薄葉紙の製造方法。
In the inter folder, in the manufacturing method of household sanitary thin paper, each continuous sheet is rewound from a winding roll obtained by winding a base paper made of pulp fiber with a predetermined width, and these are folded and stacked to produce a product.
For the base paper in the paper making process, as an active ingredient, at least one of wet paper strength agent, softener and carboxymethylcellulose is added in advance as an additive,
A roll by a gravure roll by adjusting a pH of a moisturizing chemical solution different from the additive as an active ingredient to 5.0 to 6.0 as an active ingredient between unwinding and folding stacking steps in the interfolder A method for producing a sanitary thin paper for home use, characterized in that the chemical solution is continuously applied by transfer and then impregnated with the chemical solution by a pressing device so that the chemical solution content per sheet unit volume is 12 to 45 mg / cm 3. .
有効成分における湿潤紙力剤、柔軟剤およびカルボキシメチルセルロースの少なくとも一種の比率を3.0〜4.5重量%とし、
有効成分における薬液の比率を95.5〜97.0重量%とする、請求項1記載の家庭用衛生薄葉紙の製造方法。
The ratio of at least one of wet paper strength agent, softener and carboxymethyl cellulose in the active ingredient is 3.0 to 4.5% by weight,
The manufacturing method of the household sanitary thin paper of Claim 1 which makes the ratio of the chemical | medical solution in an active ingredient 95.5 to 97.0 weight%.
JP2011249729A 2004-08-31 2011-11-15 Manufacturing method of household sanitary thin paper Active JP5425867B2 (en)