CS237784B1 - Složení práškového drátu - Google Patents

Složení práškového drátu Download PDF

Info

Publication number
CS237784B1
CS237784B1 CS817563A CS756381A CS237784B1 CS 237784 B1 CS237784 B1 CS 237784B1 CS 817563 A CS817563 A CS 817563A CS 756381 A CS756381 A CS 756381A CS 237784 B1 CS237784 B1 CS 237784B1
Authority
CS
Czechoslovakia
Prior art keywords
manganese
nickel
welding
calcium
silicon
Prior art date
Application number
CS817563A
Other languages
English (en)
Other versions
CS756381A1 (en
Inventor
Vladimir J Zusin
Vjaceslav I Cernoivanov
Gennadij N Vainer
Anatolij N Kabanec
Viktor A Muratov
Vladimir K Gorodkov
Raif S Chasanov
Original Assignee
Vladimir J Zusin
Vjaceslav I Cernoivanov
Gennadij N Vainer
Anatolij N Kabanec
Viktor A Muratov
Vladimir K Gorodkov
Raif S Chasanov
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Vladimir J Zusin, Vjaceslav I Cernoivanov, Gennadij N Vainer, Anatolij N Kabanec, Viktor A Muratov, Vladimir K Gorodkov, Raif S Chasanov filed Critical Vladimir J Zusin
Priority to CS817563A priority Critical patent/CS237784B1/cs
Publication of CS756381A1 publication Critical patent/CS756381A1/cs
Publication of CS237784B1 publication Critical patent/CS237784B1/cs

Abstract

Složeni práškového drátu se týká svařování zvláště materiálů používaných pro svařování a navařování hliníkových slitin. Cílen je zvýšení odolnosti proti opotřebení kovu sváru při zvýšených teplotách. Stanovený cíl se dosahuje tín, že v sestavě práškového drátu, především prs svařování hliníkových slitin, skládající se z hliníkového obalu a z náplně, zahrnující měď, křaalk a složku obsahující ziřkon, nápln dále obsahuje mangan a nikl a jako složku obsahující zirkon - fluorozirkonát vápníku, při tomto poměru složek ve hmotnostních %: ϋΓ* °·3 8Ž 2·5 křemík 13,1 až 24 fluorozirkonát vápníku 0,1 až 5 mangan 0,8 až 3 nikl 0,7 až 5 hliníkový obal zbytek.

Description

(54) Složení práškového drátu
Složeni práškového drátu se týká svařování zvláště materiálů používaných pro svařování a navařování hliníkových slitin.
Cílen je zvýšení odolnosti proti opotřebení kovu sváru při zvýšených teplotách.
Stanovený cíl se dosahuje tín, že v sestavě práškového drátu, především prs svařování hliníkových slitin, skládající se z hliníkového obalu a z náplně, zahrnující měď, křaalk a složku obsahující ziřkon, nápln dále obsahuje mangan a nikl a jako složku obsahující zirkon - fluorozirkonát vápníku, při tomto poměru složek ve hmotnostních %:
ϋΓ* °·3 8Ž 2·5 křemík 13,1 až 24 fluorozirkonát vápníku 0,1 až 5 mangan 0,8 až 3 nikl 0,7 až 5 hliníkový obal zbytek.
Η3Ο0ρβΤΘΗΗΘ OTHOCHTCH Κ 0Β8ρΚβ, 3 qaCTHOCTH Κ Μ3Tepnanau, npuueHHeuuu ana caapKH h HanaaBKH θπβμηηηθbux cnaabob.
Η3ΒβοτβΗ cociaB cBapoqHoro uaTepHana /1/, coaepaamero caeay®insie κομποηθητη, Bec.%:
Haas 4,8-5,8
KpeMHHít 1,2-2,0
Mama» t 0,25-0,45
Οποβο 2,7-3,5
AanuHHHft OcxaabHoe.
ΟτξΗΘΚΟ H3B6CTHUtt CBapOMHHÍt ΜΘΤβρΜΘΠ Ο0βΟΠθΗΜΒ3ΘΤ
HanocTaiOMHy» h3hococtoí!koctii Meiaaaa osa.
Hanóoaee Óbhskhm κ ΗΒΟόρβτβΗίπο no cocTaBy ηβληθτch nopomKOBafl προΒΟποκβ /2/, cocTOHmaa xs aaDUHHBeBOtl oúoaonKH η ιπηχτη, BKaBnaBnaň caeayBtnHe κομποηθητη, Bec.%:
ΚρβΜΗΗϋ 4,6-5,9
Marniia 0,45-0,9
KounoH9HT,coaepxa[HHít mipsomilt 0,2-0,3
Mas* 0,2
ΑΒΒΜΗΗΗβΒβΗ oóoaoMKa Ocxaa&Hoa.
HeaOCTaTKOM Η3ΒβΟΤΗθΒ ΠΟρΟΟΚΟΒΟΚ ΠρΟΒΟΠΟΚΗ ΗΒΙΙΗΘΤCH ΗΗ3Κ3Η Η3ΗΟΟΟΟΤΟΒΚΟΟΤΒ ΜβΤ9ΛΠ3 Οθ ΠρΗ ΠΟΒΗΠΙβΗΗΗΧ TeunepaTypax.
ΠβΤΙΒ Η300ρβΤβΗΗΗ - ΠΟΒΗΒΙβΗΗβ H3H0C0CT0ÍÍK0CTH M6T3JIJia maa πρκ πθΒΗΐπβΗΗΗχ TeMnepaTypax.
HenB Aocraraeicfl Teu, πτο τηχτθ ΑΟποπΗΗΤβπΒΗΟ coaepxHT uapraaeu η ηηκθαβ, a b KaqecTBe KOunOHema, coaepxamero ηπρκοΗΗΒ, - φτορφίρκοΗβτ najma, πρκ caeays)meM ΟΟΟΤΗΟΟΙΘΗΗΗ ΚΟΜΠΟΗβΗΤΟΒ, ΒβΟ.%ϊ
Meas 0,3-2,5
KpeMHHa 13,1-24
ΦΤΟρΠϋρΚΟΗβΤ K3JIIIH 0,1-5 MapraHea 0,8-3
Ηηκθλβ 0,7-5
Απμμηηηθβθη otfojioqKa OcTajr&Hoe.
MeaB BBOaHTCH B COCTaB nOpOBIKOBOa ΠρΟΒΟΠΟΚΗ B npeaeaax 0,3-2,5% ana ποβηιπθηηη xaponpoqHOCTH h H3HOcocToa koctsí HawiaBJíeHHOro Meianna πρκ noButneHHHX TeMnepaTypax. Πρκ coaepxaHHH Mean b cocias nopomKOBoro aaeKTpoaa 0,3% h Meaee βιιηηηηθ ee Ha Meiajia HaimaBKH He3HaqHTeai>HO.
C yBejmqeHHeM coaepxaHHH MeaH ao 2,5% β πιηχτθ ποροαικοBoa npOBOJiOKH MeTajui HanaaBKH oóaaaaeT nOBHineHHHMH npOqHOCTHHMH ΧθρθΚΤβρΗΟΤΗΚβΜΗ ΠρΗ ΑΑΗΤΘΠΒΗΟΜ Η3ΓρβΒΘ ao TeunepaTyp +300-400°C. 9to ofoacHaeTca Teu, qTO uaai» npn coaepxaHHH ao 2,5% yqacTByeT β ποβηπθηηη uexaTOUHoa CBH3H TBepaoro pacTBopa, coaepxamero uapraHen. Kpoue Toro, npa pacnaae TBepaoro pacTBopa οποχηογο no cocTaBy cnaaBa otipasytoTca BHcnepcHue qacTHuu φβ3Η T(Al^MnOu) , κοτορΗθ yqaciBywT b ooeaaHHH uhkpoΓβΤβρΟΓβΗΗΟΟΤΗ BHyTpH 3βρβΗ ΤΒβρΚΟΓΟ paCTBOpa, ΗΤΟ saipyaHaeT ΑβφορΜβΗΗ». Μ30ητοπηθη ueas yqacTByeT β o6ρ330Β3ΗΗΗ ΗΗΚΘΑΒΟΟΑβρΧβΑβΒ φθ3Η T (AlgGu^Ni) , KOTOpaa BpHCT3JiJiH3yeTca β pasaeTBneHHoB φορΜβ, ee qacTmm» pacnonarancB no rpaHapa 3βρβΗ TBepaoro pacTBopa, dnoKHpy»T hx η T6M cauuu oóecneqHBaioT 3naqHTeni>H0e ποβηui6HH6 xaponpozHOcTH cnnaBa. CoaepxanHe uegH β ιπηχτθ nopouiKOBOít npoBOJiOKH cneayei orpaHHZHTB 50 2,5%,
Tas K3K πρκ coAepxaHHH fioaee 2,5%, b cTpyKType HanaaBKH ποπβπηθτοη $a3a CuAl2 » cnocoficTByBman OXpynZHBaHHB 0ΠΗΘΒ8, ΠΟΗΗΧβΗΗΒ Κθρρθ3ΗΟΗΗΟ0 CTOflKOCTH H, caeΖΙΟΒΘΤβΠΒΗΟ, H3HOCOCTO0KOCTH Η ΠΟΒΗΠΙβΗΗΒ CKBOHHOCTH K ΟόΈΘΜΗΗΜ Η3ΜθΗΘΗΜΗΜ.
ΚρβΜΗΗβ, BB05HUHÍÍ B C0CT3B nOpOIDKOBOfl ΠρΟΒΟΠΟΚΚ b npeaeaax 13,1-24%, cnocoficiByeT οηηχθηηβ κθ3φφΗΕ(Η6ΗTa πΗΗββΗΟΓΟ pactnupeHHH, noBHtnaaT TBepaociB h yBenazHBaei h3hococtoHkoctb MeTaaaa ππθβκη πρκ ποβηιπθηηηχ TeMnepaTypax.
lípu coaepsaHHH κρβΜΗΗΗ Huse 13,1% β οοοτθβο dimxtu nopotiiKOBOň προΒοηοκΗ HanaaBaeHHHít MeTaaa ofiaaaaeT noHHX6HHHUH npOqHOCTHHUH Χ3ρ3ΚΤβρΜ0ΤΗΗ3ΜΗ, ΠΟΒΗΠβΗΗΗΜ κοθφφΗΗΗβΗΤΟΜ jiHHeílHOiO pacmHpeHHa, a caeaoBaieaBHO,
Η HH3KHMH CBOflCTBaUH ΠΟ «apOnpOqHOCTH. ΠρΗ ΟΟ^βρΧβΗΗΗ ΚρβΜΗΗΗ Β 111ΗΧΤΘ ΠΟρΟΒΚΟΒΟΑ ΠρΟΒΟΠΟΚΗ όΟΠΘβ 24% ΜβΤβΠΒ HanaaBKH ΠΟΖξΒβρΧβΗ TpenjHH00fip330B8HHB ΟΤ ΗΗΚΠΗΗβΟΚΗΧ HanpflXeHHÍt Η 0XpynZHB3HHB, ΗΤΟ ΟΗΗΒΘΘΤ ΠρΟΗΗΟΟΤΗΗβ xapaKTepHCTHKH.
HupKOHHň Β C0CT3B fflHXTU ΠΟρΟΗΗΟΒΟβ ΠρΟΒΟΒΟΚΗ ΒΒβίξβΗ Β ΒΗΒ6 φΤΟρΗΗρΚΟΗΘΤβ Κ8ΒΗΗ, 3Τ0 πρΗΒΟίΗΤ Κ ΜΟΖξΗφΗηΗρΟΒΘΗΗΒ Η8ΠΒ3ΒΒβΗΗ0Γ0 ΗβΤβΒΠΘ Η ΠΟΒΗΠΙβΗΗΒ 6Γ0 ΠΠΟΤΗΟΟΤΗ, ΠΤΟ ΟόθΟΠβΜΗΒββΤ γΒΘΒΗΗβΗΗβ H3H0C0CTOflKOCTH uaTepnaaa πρκ ποβηιιιθηηηχ TeMnepaTypax 3a cqeT fioaee paBHOuepHoro pacnpeaeaeHHH TBepztux βκββπθηηΑ no ofiseuy ηθπβθββθηηογο MeTaaaa.
0fipa3ywie b HannasneHnoM ueTaaae ηητθρμθτθβπηζιη 8BBMHHHH H impKOHHH ΠΟΒΗΒβΒΤ XapOnpOZHOGTB 0ΠΠ8Β8.
ΒΒθίβΗΗβ φτορπΗρκοΗβτβ κθπηη cnocoficTByei 0ΤθΰΗΠΗ38mra nponecca HanaaBKH, ynyqmeHHe cBapoqHO-TexHoaorHqeckhx xapaHTepHCTHK nyru, cnocoficiByeT ofipaaoBaaHB toh237784 κογο cjioh nuiaHOBofi οδοποηκΗ, κοτορβΗ npesoxpaHfleT CBapoqHyw BaHHy οτ B03AeítCTBHH B03nyxa.
ΚρΟΜΘ 3Τ0Γ0, UHpKOHHfi ΟΗΗΧββΤ CKJIOHHOCTh ΟΠΛΘΒΘ Κ ΓΟρΗΗΗΜ ΤρθφΙΗΘΜ, npOH3BOAHT ΑβΓ333ΙξΗΒ ΟΠΛΘΒΘ, ΠΟΒΗΠΙΘβΤ nnoTHOCTB HannaBKM, γοτρβΗΗβτ nopootípa3OBaHne.
3φφβΚΤ ΜΟΑΗφΗΕρκρΟΒΘΗΗΗ ΜβΤΘΟΘ H3ÓHBíaeTCH ΠρΗ COAepxaHHH φΤΟρΑΗρΚΟΗΒΤΘ K3JIHH Β ΠΙΗΧΤβ ΠθρθΠ1ΚθΒΟ0 ΠρΟΒΟΠΟΚΗ 0,1%. 3ΤΗΜ OtíyCJIOBJíeH ΒΗΧΗη'8 ΠρβΖζβΠ ΟΟΖξβρΧβΗΗΗ φΤΟρΠΗρΚΟΗΘΤβ ΚΘΠΠΗ. ΣΒβΠΗ^βΗΗβ ΟΟΠβρΧΘΗΗΗ φΤΟρΗΗρΚ0Η8Τ3 Κ3ΠΗΗ ΒΗΠ16 5% Β ΠΙΗΧΤβ ΠΟρΟΙΠΚΟΒΟΑ ΠρΟΒΟΠΟΚΗ ΟΠΟcodcTByei ποΒΗΐπβΗΗΒ οκποηηοοτη MeTanna ηθπηθβκη κ oxpynqoaHHi). Β CBH3H c 3Τημ coaepxaHHe φτορπκρκοΗβτθ KaΠΜΗ Β ΠΙΗΧΤβ ΠΟρΟΙΠΗΟΒΟίΙ ΠρΟΒΟΠΟΚΗ (5θϊΙββ 5% Ηβρ3ΠΗ0Η3ΠΒHO.
MapraHep β npenenax 0,8-3% β coqeTaHHH c κρβΜΗΗβΜ Η ΜβΖζΒΒ Β yK333HHHX ΠρβΠβΠΘΧ ΠΟΒΗΠΙΘβΤ ΤΒβρξΟΟΤΒ Η ΠρΟΠhoctb HannaBJíeHHoro MeTanna πρκ πΟΒκπιβΗΗΗΧ TeunepaTypax
CosepxaiHie β πιηχτθ ποροπικοΒΟίί προΒοηοκκ MapraHpa ΜβΗΒΙΠβ 0,8% Ηβ 0Κ33ΗΒ3βΤ ΒΠΗΗΗΗΗ Ηθ XapaKTepHCTHKH XapO npoqHOCTH Η H3H0C0CT0&K0CΤΗ ΜβΤΒΠΠΘ Η3ΠΠ8ΒΚΗ. ΠρΗ COnepxaHHH MapraHua βηνθ 0,8% η no 3% θτομη MapraHna, HaxoAHCB β κρΗοτθππκπβοκοΗ ρβπιβτκβ TBepAoro paciBopa, cnocotfcTByioT nepepacnpeneneHHB βθπθητηηχ οηβκτροΗΟΒ a tom ob npyrnx 3ΗβΜβπτοΒ. 3το cnocotícTByeT yBenHqeHHB MexaTOMHOfi CBH3H, ΠΟΗΗΧβΗΗΒ ΚΟθφφΗΐχΗΘΗΤθ C3M0ZIH$$y3HH 3ΠΒΜΗΗΗΗ Η ΤβΜ C3MHM ΠΟΒΗΙΠβΗΗΒ XapOnpOqHOCTH H H3H0cocTOfiKOcra cnnasa. Οαηθκο γΒβπΗηβΗΗβ conepxaHHH MapraHIja ΒΗΙΠ6 3% Β ΠΙΗΧΤβ ΠΟρΟΠΙΚΟΒΟβ ΠρΟΒΟΠΟΚΗ HetínaroπρκΗΤΗΟ cKaabiBaeTca Ha ο3ηητ3ρηο-γηγηθηηπ6οκηχ ycnobhhx nponecca HannaaHH.
ΒΒβΑβΗΗβ 0,7-5% ΗΗΚβΠΗ ΜβΠΟ Η3ΜΘΗΗ6Τ ΜβΧβΗΗΠβΟκηθ CBOflcTBa cnnaBa πρκ κομηθτηοΚ leanepasype, ho 3aμθτηο noBMinaeT ero xaponpoqHOCTB πρκ ποΒΗΐπβΗΗΗΧ τβΜnepaTypax. 3to ούΒΗΟΗΗβτοπ τβΜ, qto HHKejiBconepxaqaH φθ33 cnocotícTByei ynpoqHeHHB rpaHHH 3βρβπ TBepnoro paciBopa. lípu coqepxaHHH ηηηθπη βηπιθ 5% β ποροοκοΒΟβ ΠρΟΒΟΠΟΚΘ yBenUMHBaeTCH ΤΒβρΠΟΟΤΒ ΗβΠΠΰΒΚΗ Η CHUOHHOCTB κ OXpynqHBaHHK).
Tipu COZtepxaHHH ΗΗΚΘΗΗ ΗΗΧβ 0,7% Η3Μ6ΗβΗΗβ CBOttCTB aaponpoMHocTH h h3hococtoí1kocth πρπ ποβειιπθηηηχ τθμπθpaiypax ηθ HatínionaeTCH.
CociaBu nopooiKOBux προβοποκ npeíCTaBneHH b Ta<5jiHpe 2.
CBOftcTBa HanjiaBJíeHHoro «eianna tipu ποβηώθηηηχ TeMnepaiypax πρωβίβΗΜ b latínHije 2«
B KaqeCTBe riOpOUIKOBHX íipOBOJIOK Μ3Γ0Τ3ΒΠΜΒ3 JIHCL Π6ΗΤΗ CeqeHHeM 7 X 1,5 UU. ΠΟρΟΙΠΚΟΒΗΘ JISHIEI Η3Γ0Τ8ΒjioaocL Ha CTaHaapTHOu ofiopynoBaHHH. HaruiaBKy ocynecTBjíflBT Ha cneayioineM pexHMe: Icg =200-250A,
Ux =15-17 B, Vcg =8 u/q.
Ws nojiyqeHHux πθηηηχ bhaho, hto HazĎojiee h3hococtoHhhmh cBoftcTBauu π pa ποβηιπθηηηχ TeMnepaiypax otínanaei cocTaB 5, πρηηητηΒ sa onTnuajiBHHfl.
ΠρΗΜδΗβΗΜβ ΖξθΗΗΟΓΟ ΠΟρΟΙΠΚΟΒΟΓΟ aaeKTpoaa ΤΟΠΒΚΟ 5JiH HannaBKH nopmHea nBHraieneň πο3βοπηθτ 3HaqHienBho yBennqHTB cpoK hx sKcnnyaTauHH 3a cqeT ποβμπθηηη H3H0C0CT0ítK0CTH.
Tatíjraqa I
KounoaeHTu COCTaB nOpOfflKOBHX ÍIPOBOJIOK
I (HhshhA npeaen) 2 (BepxHHÍt npeaen) 3 (ΟπτημθηβηηΒ)
KpeuHHft 13,1 24 13,3
Mesb 0,3 2,5 1,4
ΗΗΚβΠΒ 0,7 5. 2,5
UapraHeq 0,8 3,0 Λ3
ΦΤΟρηΒρΚΟΗΘΤ
Κ&ΠΗΗ 0,1 5,0 0,9
ATOMiiHiíeBaa
odonoqKa OcTaonoe
Tadmma 2
ΟοοτβΒΗ no- Teíinepa- Οτηοοητθ- TsepaocTB Koafo.· pouiKOBHX Typa hc- Han H3HO- HannaBnea- jiaaeŽHOi προβοποκ πητθηηΑ, cocioft- ηογο MeTán- pacmupeHafi oc kootb na ΗΒ,κγ/μμ
I(hhshh0
npeaen) 2(ΒβρΧΗΒ0 300 Ι,Ι 75,5 4,15
npeaen) 3(θΠΤΗΜ3ΠΒ- 300 1,8 89,7 3,95
HU0) 300 2,2 98,3 2,45
ΠρΟΙΟΤΗΠ 300 ι,ο 64,8 9,80
ΦΟΡΜΪΛΑ Η3ΟΒΡΕΤΕΗΜΗ
COCTaB ΠΟρΟΠΙΚΟΒΟδ npOBOJIOKH, npeHMyHeCTBeHBO flJIH CBapKM 8 JliOMHHHQBtíX CnnaBOB, COOTOHIHH0 H3 3)ΙΙΟΜΗΗΗ6ΒΟ0 oÓojiobkh h oihxtu, BKJitoqaiomeíl Ment, KpeUHHit u homπΟΗβΗΤ, coaepxatnHíí phpkohhK, OTJiHqaiotUHlíCfi tom, bto ,
C peJIM) ΠΟΒΗΙΠβΗΗΗ H3HOCOCTO0KOCTH ΜβΤ3ΠΠ8 ΙΠΒΘ ΠρΗ ΠΟΒΗΐπβΗΗΗΧ TeMnepaiypax, πιηχτθ nonojiHHíejiBHO conepauis uapraHeu a hhkqjib, a b KaqecTBe κομποηθητθ, coaepxamero mipKOHna, - φτορρΗρκοΗβτ κηιιηη, πρκ cjienyameii COOTΗΟΠΙβΗΗΗ Κ0ΜΠ0ΗβΗΤ3, Bec.%:
Mezti. 0,3-2,5
KpeuHHft 13,1-24
ΦΤΟρίίΗρΚΟΗΘΤ
K3JIHH 0,1-5
MapraHep 0,8-3
ΗιικβιΐΒ 0,7-5
A JH0MHHH6B3 H
oóojioqKa OciajiBHOe.
tíCTOqHHKH HH$OpyaiHHH, npHHHThie BO
ΒΗΗΜβΗΗβ
3KcnepTH3e: ,
1. ABTopcKoe cBHneTenBCTBO CCCP řfe 351920, KJI. C 22 C 21/16, 1969.
2. ABTopcKoe οΒΜΑθτβΑΒΟΤΒΟ CCCP Hs 228823, kji. B 23 K 35/28, 1967 (προτοτΗπ).
ΠρΗ
A Η Η O T AU Η
COCTaB ΠΟρΟΟΙΚΟΒΟϋ ΠρΟΒΟΠΟΚΗ 0TH0CHTC3 Κ ΟΒθρΚβ,
Β qaCTHOCTH Κ Μ3ΤβρΜ3Π8Μ, ΠρΗΜβΗΗβΜΗΜ 5ΠΗ 0Β3ρΚΚ Η ηθππθβκη amoMHHíieBMx cnnaBOB.
ΠβΛΒ Η300ρβΤβΗΗΗ ΠΟΒΗΟΘΗΗβ H3H0C0CI0ÍÍKCCΤΗ Μβτθππβ ο a πρκ nOBHtneHHHX TeMnepaTypax.
ΠΟΟΤΘΒΠβΗΗβΑ ΙξβΠΒ ΗΟΟΤΗΓθβΤΟΗ ΤβΜ, tJTO Β ΟΟΟΤΘΒβ ΠΟρΟΙΠΚΟΒΟβ ΠρΟΒΟΠΟΚΗ, ΠρβΗΜγΠΙβΟΤΒβΗΗΟ ΗΠΗ CBapKH ΘΠΒΜΗΗΗ6ΒΗΧ CÍIHaBOB, COCTOHIHeíl Η3 3ΠΒΜΜΗΗ6Βθϋ ΟόΟΠΟηΚΚ Η ΜΗΧΤΗ, BKJHOqafOmeK ΜβΖξΒ, ΚρβΜΗΗίί Η ΚΟΜΠΟΗβΗΤ» ΟΟΖξβρxamHít φίρΚΟΗΗϋ, OIHXTa ΛΟΠΟΠΗΗΤβΠΒΗΟ COflepXHT ΜβρΓβΗβη η HHítenL, a β KaqecTBe κομποηθητη, co^epsamero ÍÍHpKOHHÍt,- φΤΟρίίΗρΚΟΗΘΤ ΚΘΠΗΗ, ΠρΗ GΠβflytOΒξβΜ COOTHOtaeHHH ΚΟΜΠΟΗ6ΗΤΟΒ, Bec.$í
μθπβ 0,3-2,5
ΚρβΜΗΗίί 13,1-24
φΤΟρρπρΚΟΗβΤ
κθπηη 0,1-5
MapraHeu 0,8-3
ΗΗΚβΠΒ 0,7-5
3Η10ΜΗΗΗ6Β3Η
odonoqKa ocTaaiHoe

Claims (1)

  1. PŘEDMĚT VYNÁLEZU
    Složení práškového drátu, zejména pro svařování hliníkových slitin, sestávající z hliníkového obalu a náplně, obsahující měň, křemík a složku obsahující zirkon, vyznačující se tím, že pro zvýgení odolnosti proti opotřebení kovu sváru při zvýšených teplotách náplň obsahuje mangan a nikl a jako složku obsahující zirkon -fluorozinkonát vápníku, při tomto poměru složek ve hmotnostních %:
    měň 0,3 ež 2,5 křemík 13,1 až 24 fluorozinkonát vápníku 0,1 až 5 mangan 0,8 až 3 nikl 0,7 až 5 a hliníkový obal zbytek.
    t
    Uznáno vynálezem na základě výsledků expertizy, provedené Státním výborem pro vynálezy
CS817563A 1981-10-13 1981-10-13 Složení práškového drátu CS237784B1 (cs)