CN110003767A - A kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and the preparation method and application thereof - Google Patents

A kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and the preparation method and application thereof Download PDF

Info

Publication number
CN110003767A
CN110003767A CN201910212921.7A CN201910212921A CN110003767A CN 110003767 A CN110003767 A CN 110003767A CN 201910212921 A CN201910212921 A CN 201910212921A CN 110003767 A CN110003767 A CN 110003767A
Authority
CN
China
Prior art keywords
environment
mould proof
friendly solvent
floor paint
free
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201910212921.7A
Other languages
Chinese (zh)
Inventor
王永
李华刚
胡中源
董立志
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hebei Chenyang Industry and Trade Group Co Ltd
Original Assignee
Hebei Chenyang Industry and Trade Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hebei Chenyang Industry and Trade Group Co Ltd filed Critical Hebei Chenyang Industry and Trade Group Co Ltd
Priority to CN201910212921.7A priority Critical patent/CN110003767A/en
Publication of CN110003767A publication Critical patent/CN110003767A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses anti-skidding mould proof floor paints of a kind of environment-friendly solvent-free and the preparation method and application thereof, and by weight percentage, raw material includes following components: epoxy resin 30~60%, color sand 30~50%, auxiliary agent 1~4%, curing agent 5~20%.The anti-skidding mould proof floor paint of environment-friendly solvent-free provided by the invention not only remains existing floor tile advantage easy for construction, and accomodation ground is made to have color sand effect, decorative surface, skid resistance and artistry, opposite toilet often with the color unicity of floor tile, there are seam, shelter evil people and countenance evil practices, ground is easily sliding and poor waterproof properties the disadvantages of, have a very significant increase.

Description

A kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and the preparation method and application thereof
Technical field
The present invention relates to floor paint fields, more particularly to a kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and its preparation side Method and application.
Background technique
As the improvement of people's living standards, people constantly pursue on the surface decoration materials such as toilet, kitchen, balcony It is superior, as bright as a sixpence vitrified tile, floor tile are largely selected, fashion, noble purpose are had reached.However, these flooring boards Once material is moist or ponding, and the accidents such as be easy to slip in active procedure, in the bathroom, especially soapsuds, Under the effects of shower cream, shampoo, it is easier to which slip accident.
Currently, ordinary toilet floor treatment in the market is still to be laid with based on floor tile, although easy for construction, price is just Preferably, but the color of floor tile it is single, there are seam, easily shelter evil people and countenance evil practices, ground is easily sliding and poor waterproof properties, and the later period be difficult to clean up it is dry Only, it is difficult to renovate.
Therefore, anti-skidding, the mould proof problem for how improving accomodation ground, has caused the concern of people.
Summary of the invention
Technical problem to be solved by the present invention lies in provide a kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and its preparation Method and application make floor paint on the basis of keeping original floor tile feature easy for construction, increase the mould proof of ground, skid resistance, Artistic effect, the feature of environmental protection, and reduce construction cost.
To achieve the above object, the present invention provides following schemes:
The present invention provides a kind of anti-skidding mould proof floor paint of environment-friendly solvent-free, by weight percentage, raw material include below at Point:
Preferably, the epoxy resin is bisphenol A epoxide resin.
Preferably, the color sand is suspension lightweight circle color sand.Suspension lightweight color sand can float on the upper layer of floor paint, and one Aspect enhances antiskid effect, and enhancing is decorative, on the other hand, can increase the weatherability of terrace.
Preferably, the partial size of the suspension lightweight circle color sand is 120-200 mesh.
Preferably, the curing agent is polyamide.It is highly preferred that the curing agent is polyamide YD8216, The curing agent contains admittedly for 100%, is free of organic volatile, and the feature of environmental protection is good, and after mixing with epoxy resin, curing rate is fast, solidifies Hardness is high, obdurability is good, chemical resistance is strong, and compact in paint film after solidification, and gap is not present, and bacterium can not adhere to and life It deposits, there is good anti-mold effect.
Preferably, the auxiliary agent includes dispersing agent, defoaming agent and rheology modifier.It is highly preferred that dispersing agent is BYK104S, defoaming agent BYK-141, rheology modifier BYK-410.Rheology modifier BYK-410 is by being precipitated the crystallization bodily form Its thixotropy is realized at tridimensional network, also provides for superior anti-settling, resist sagging performance.When environment-friendly solvent-free is anti-skidding When mould proof floor paint stores, rheology modifier BYK-410 is held suspension lightweight circle color sand using tridimensional network, effectively It prevents from settling, while viscosity rises, and when construction, due to the shearing force certain to system, the net of rheology modifier BYK-410 Shape is destructurized, and viscosity declines rapidly, can reach construction requirement, and after shearing force disappears, this reticular structure is in several seconds It can establish, suspension lightweight circle color sand can be made not settle and can be uniformly distributed in system.
The present invention also provides the preparation method of the anti-skidding mould proof floor paint of the environment-friendly solvent-free, the preparation method packet It includes: epoxy resin and auxiliary agent being added in dispersion machine, stirs evenly, then color sand is added in dispersion machine, be uniformly mixed, Component A is formed, curing agent is added in component A, the anti-skidding mould proof floor paint of the environment-friendly solvent-free is uniformly mixing to obtain.
Preferably, after epoxy resin and auxiliary agent being added to dispersion machine, the revolving speed of dispersion machine is adjusted to 800- The revolving speed of dispersion machine is adjusted to 400-600rpm after color sand is added by 1000rpm.Be added color sand after, can not high speed dispersion, prevent Only the structure of suspension lightweight circle color sand is destroyed.
The present invention provides the anti-skidding mould proof floor paint of environment-friendly solvent-free and is preparing toilet, balcony, in the terrace of kitchen Application.
It is uniform to produce fluidised form using suspension lightweight circle color sand, simultaneously using the auxiliary agent of control color sand sedimentation by the present invention The anti-skidding mould proof floor paint of environment-friendly solvent-free house ornamentation use in toilet, construction technology identical with traditional terrace, produce paint film cause The naked leakage of close, part color sand in surface of the paint film, reach the anti-skidding synergy with anti-ponding, mildew proof, while it is again easy to clean Floor paint assigns film simultaneously with the texture of art, and properties are very comprehensive.
Bisphenol A epoxide resin contains function monomer, and amido therein can reduce or eliminate the organic contamination in air Object, therefore toilet air quality can be improved.Adjuvant used and curing agent is environment-friendly materials in the present invention, will not be to body Harm is generated, and construction cost is lower.
Be added suspension lightweight circle color sand floor paint do not contain any dyestuff, have nontoxic, tasteless, wear-resisting, waterproof, Anti-corrosion, anticorrosive, acid and alkali-resistance, it is uprising shine, the features such as lucuriant in design, tone is soft, three-dimensional sense is strong, cohesive force is strong, non-discolouring, i.e., Make to change colour by the flushing of the liquid such as shampoo, bath foam.The addition of color sand makes floor paint have stronger gas permeability, Enhance the anti-mold effect of floor paint.
Specific embodiment
It is clearly and completely described below in conjunction with the technical solution in the embodiment of the present invention, it is clear that described reality Applying example is only a part of the embodiment of the present invention, instead of all the embodiments.Based on the embodiments of the present invention, this field is general Logical technical staff every other embodiment obtained without making creative work belongs to what the present invention protected Range.
In order to make the foregoing objectives, features and advantages of the present invention clearer and more comprehensible, With reference to embodiment The present invention is described in further detail.
Embodiment 1-6
By weight percentage, including following component:
The preparation method of the anti-skidding mould proof floor paint of embodiment 1-6 environment-friendly solvent-free: according to it is described proportion by epoxy resin with Auxiliary agent is added in dispersion machine, is adjusted the revolving speed of dispersion machine, is stirred under 800-1000rpm revolving speed, will then be suspended Lightweight circle color sand is added in dispersion machine, is sufficiently mixed uniformly under 400-600rpm revolving speed, is formed component A;By curing agent plus Enter into component A, stirs to obtain the anti-skidding mould proof floor paint of the environment-friendly solvent-free.
Environmentally friendly auxiliary agent in embodiment 1-6 includes dispersing agent, defoaming agent, rheology modifier, and wherein dispersing agent is BYK104S, defoaming agent BYK-141, rheology modifier BYK-410, environment friendly curing agent are polyamide YD8216,
The composition and ratio of the anti-skidding mould proof floor paint of embodiment 1-6 environment-friendly solvent-free are shown in Table 1.
The component of comparative example 1-3 is shown in Table 1.The curing agent of comparative example 1 is diethylenetriamine, the rheology modifier of comparative example 2 For fumed silica, other auxiliary agents are same as Example 1.
Comparative example 3 is to add the floor paint of low dose of color sand, remaining component is same as Example 1.
Table 1
Paint film property is tested, paint film property is tested according to GB/T22374-2008 terrace coating material, as a result such as table 2 It is shown.
Table 2
Above-mentioned testing result shows that paint film intensity prepared by the present invention is high, and wearability is good, and paint film property reaches GB/ T22374-2008 related request.The curing agent of comparative example 1 changes, and the rheology modifier of comparative example 2 changes, terrace The anti-skid wearable performance of paint has to be declined to a certain degree, a degree of blistering, peeling phenomenon occurs.It is main used in the present invention Agent and auxiliary agent produce synergistic effect, enhance the anti-skidding fungicidal properties of floor paint, and comparative example 3 is to add the ground of low dose of color sand Level ground paint, anti-skid factor significantly reduce.
The fungicidal properties of testing example 1-6 and comparative example 1-3: it according to HG/T 3950-2007, is examined using method for adhering film The coating fungicidal properties is surveyed, embodiment 1-6 reaches six kinds of Candida albicans and aspergillus niger etc. the comprehensive mould suppression rates of killing as the result is shown It is respectively as follows: 99.9% and 99.9% to 0 grade, while to the suppression rate of killing of staphylococcus aureus and Escherichia coli, 1-3 pairs of comparative example Six kinds of Candida albicans and aspergillus niger etc. the comprehensive moulds suppression rates of killing are respectively II grade, II grade and not up to standard, to Staphylococcus aureus The suppression rate of killing of bacterium and Escherichia coli is respectively as follows: 60.5% and 64.4%, 55.5% and 54.4%, 50.5% and 47.4%.
Workability test is done, is found: compared with traditional toilet floor tile, art effect of this product rich in cubic appearance Fruit, it is mould proof, antiskid effect is excellent.
Bisphenol A type epoxy resin is due to its special construction, and under the irradiation of sunlight, phenyl ring is easily converted to quinoid knot Structure makes paint film turn yellow, and is also easy to produce powder phenomenon-tion.The light that bisphenol A type epoxy resin can be improved in the color sand of addition large dosage is stablized Property, powder phenomenon-tion will not occur prolonged application, so that the floor paint is achieved the effect that photostability, even if when long Between use, color will not change.It is existing that within 3 years use time dusting does not occur for the floor paint of embodiment 1-6 As slight dusting occurs in 6 months for the floor paint of comparative example 3, and powder phenomenon-tion is serious in 12 months.
In the selection of auxiliary agent, using the auxiliary agent of environment-friendly solvent-free, common solvent type epoxy finishing coat construction gas is avoided Highly seasoned, the defect of big, the serious damage construction personnel's health of toxicity has reached the requirement of environmental protection.
Embodiment described above is only that preferred embodiment of the invention is described, and is not carried out to the scope of the present invention It limits, without departing from the spirit of the design of the present invention, those of ordinary skill in the art make technical solution of the present invention Various changes and improvements, should all fall into claims of the present invention determine protection scope in.

Claims (9)

1. a kind of anti-skidding mould proof floor paint of environment-friendly solvent-free, which is characterized in that by weight percentage, raw material include below at Point:
2. the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 1, which is characterized in that the epoxy resin is double Phenol A epoxy resin.
3. the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 1, which is characterized in that the color sand is to suspend gently Matter circle color sand.
4. the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 3, which is characterized in that the suspension lightweight is round The partial size of color sand is 120-200 mesh.
5. the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 1, which is characterized in that the curing agent is polyamides Polyimide resin.
6. the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 1, which is characterized in that the auxiliary agent includes dispersion Agent, defoaming agent and rheology modifier.
7. the preparation method of the anti-skidding mould proof floor paint of environment-friendly solvent-free described in claim 1, which is characterized in that by epoxy resin It is added in dispersion machine, stirs evenly with auxiliary agent, then color sand is added in dispersion machine, be uniformly mixed, form component A, it will Curing agent is added in component A, is uniformly mixing to obtain the anti-skidding mould proof floor paint of the environment-friendly solvent-free.
8. the preparation method of the anti-skidding mould proof floor paint of environment-friendly solvent-free according to claim 7, which is characterized in that by epoxy After resin and auxiliary agent are added to dispersion machine, the revolving speed of dispersion machine is adjusted to 800-1000rpm, after color sand is added, by dispersion machine Revolving speed be adjusted to 400-600rpm.
9. the application of the anti-skidding mould proof floor paint of environment-friendly solvent-free described in claim 1, which is characterized in that the environment-friendly solvent-free Anti-skidding mould proof floor paint is preparing toilet, balcony, the application in the terrace of kitchen.
CN201910212921.7A 2019-03-20 2019-03-20 A kind of anti-skidding mould proof floor paint of environment-friendly solvent-free and the preparation method and application thereof Withdrawn CN110003767A (en)