CN107245287A - Anti-skidding finish paint of illusion-colour drawn grain and preparation method thereof - Google Patents
Anti-skidding finish paint of illusion-colour drawn grain and preparation method thereof Download PDFInfo
- Publication number
- CN107245287A CN107245287A CN201710618214.9A CN201710618214A CN107245287A CN 107245287 A CN107245287 A CN 107245287A CN 201710618214 A CN201710618214 A CN 201710618214A CN 107245287 A CN107245287 A CN 107245287A
- Authority
- CN
- China
- Prior art keywords
- illusion
- colour
- finish paint
- skidding
- drawn grain
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of anti-skidding finish paint of illusion-colour drawn grain and preparation method thereof, the non slip surface enamel-cover includes following component by weight percentage:Epoxy resin 20~30%;Thixotropic agents 5~10%;Color stuffing 15~30%;Auxiliary agent 3.5~5%;Color sand particle 10~20%;Curing agent 15~20%.The anti-skidding finish paint is by adding bisphenol A type epoxy resin and modified amine curing agent, then is equipped with the color sand particle of organic resin synthesis, improves the hardness and resistance to marring of epoxy material.Thixotropic agents and color sand particle are equipped with solvent-free system so that after material makes, show color sand particle, while also having uniform concavo-convex paint film, there is a good skid resistance, i.e., it is attractive in appearance and have more excellent physical property.
Description
Technical field
The present invention relates to the finish paint field of construction material, more particularly to a kind of anti-skidding finish paint of illusion-colour drawn grain and its preparation side
Method.
Background technology
Existing epoxide terrace finish paint has the following disadvantages:Hardness low (pencil hardness 2H)/resistance to marring is poor, uses one section
Time easily grows dim, and coefficient of friction is low, and skid resistance is poor, and the VOC and the feature of environmental protection of existing epoxide terrace are poor.
The content of the invention
Based on the problems of prior art, it is an object of the invention to provide a kind of anti-skidding finish paint of illusion-colour drawn grain and its system
Preparation Method, can solve that existing epoxide terrace soft, resistance to marring be poor, the problems such as growing dim, construct cumbersome of turning white after paint film abrasion.
The purpose of the present invention is achieved through the following technical solutions:
Embodiment of the present invention provides a kind of anti-skidding finish paint of illusion-colour drawn grain, including following component by weight percentage:
Embodiment of the present invention also provides a kind of preparation method of the anti-skidding finish paint of illusion-colour drawn grain, it is characterised in that for making
The standby anti-skidding finish paint of illusion-colour drawn grain of the present invention, comprises the following steps:
Each raw material is taken by the formula of the anti-skidding finish paint of illusion-colour drawn grain of the present invention;
After epoxy resin addition auxiliary agent is well mixed, thixotropic agents and color stuffing are added while stirring, 20 are disperseed at a high speed
After minute, below fineness 80um adds color sand particle and stirred mian paint is made;
Curing agent is added into above-mentioned mian paint, the anti-skidding finish paint of illusion-colour drawn grain is made after stirring.
As seen from the above technical solution provided by the invention, the anti-skidding finish paint of illusion-colour drawn grain provided in an embodiment of the present invention
And preparation method thereof, its advantage is:
By adding bisphenol A type epoxy resin and modified amine curing agent, then the color sand particle of organic resin synthesis is equipped with, carried
The hardness and resistance to marring of high epoxy material.Thixotropic agents and color sand particle are equipped with solvent-free system so that material makes
Afterwards, show color sand particle, while also having uniform concavo-convex paint film, there is a good skid resistance, i.e., it is attractive in appearance and have more excellent thing
Rationality energy.
Embodiment
With reference to the particular content of the present invention, the technical scheme in the embodiment of the present invention is clearly and completely retouched
State, it is clear that described embodiment is only a part of embodiment of the invention, rather than whole embodiments.Based on the present invention
Embodiment, the every other embodiment that those of ordinary skill in the art are obtained under the premise of creative work is not made,
Belong to protection scope of the present invention.
The embodiment of the present invention provides a kind of anti-skidding finish paint of illusion-colour drawn grain, including following component by weight percentage:
In above-mentioned anti-skidding finish paint, resin uses bisphenol A type epoxy resin.
In above-mentioned anti-skidding finish paint, curing agent uses modified fatty amine or modified polyether amine.
In above-mentioned anti-skidding finish paint, thixotropic agents are using bentonite and modified aerosil, and the consumption of each component is by unreal
The percentage by weight meter of the total consumption of the color anti-skidding finish paint of drawn grain, be respectively:Bentonite 4~5%, modified aerosil 1~
5%.
In above-mentioned anti-skidding finish paint, color sand particle uses import organic resin synthetic material.
In above-mentioned anti-skidding finish paint, the auxiliary agent includes:Defoamer, levelling agent and dispersant, the consumption of each component press illusion-colour
The percentage by weight meter of the total consumption of the anti-skidding finish paint of drawn grain, be respectively:Defoamer 0.8~1.5%, levelling agent 1.7~2.5%, point
Powder 1%.
In above-mentioned anti-skidding finish paint, the color stuffing uses titanium dioxide and filler, and the consumption of each component is anti-skidding by illusion-colour drawn grain
The percentage by weight meter of the total consumption of finish paint:Titanium dioxide 0.5~1%, filler 14.5~29%.
The embodiment of the present invention also provides a kind of preparation method of the anti-skidding finish paint of illusion-colour drawn grain, it is characterised in that for preparing
The above-mentioned anti-skidding finish paint of illusion-colour drawn grain, comprises the following steps:
Each raw material is taken by the formula of the above-mentioned anti-skidding finish paint of illusion-colour drawn grain;
After epoxy resin addition auxiliary agent is well mixed, thixotropic agents and color stuffing are added while stirring, 20 are disperseed at a high speed
After minute, below fineness 80um (to meet production technology index request) adds color sand particle and stirred mian paint is made;
Curing agent is added into above-mentioned mian paint, the anti-skidding finish paint of illusion-colour drawn grain is made after stirring.
The embodiment of the present invention is specifically described in further detail below.
Embodiment 1:
The present embodiment provides a kind of anti-skidding finish paint of illusion-colour drawn grain, including following components, and its percentage by weight is:
(1) mian paint includes:
128 epoxy resin 30%
Color sand particle 13%
Color stuffing:
Titanium dioxide 0.5%
Filler 28%
Thixotropic agents:
Bentonite 4%
Modified aerosil 2%
Auxiliary agent:
Defoamer 0.8%
Levelling agent 1.7%
Dispersant 1%
(2) curing agent:
Modified amine curing agent 19%
After taking the 128 epoxy resin addition auxiliary agent in above-mentioned mian paint well mixed, the swollen of thixotropic agents is added while stirring
The titanium dioxide and filler of profit soil and aerosil and color stuffing, after disperseing 20 minutes at a high speed, below fineness 80um, then add
Enter color sand particle and stir mian paint is made;
Modified amine curing agent is added into obtained mian paint, finish paint is made after stirring, paint film is prepared with the finish paint,
Paint film property is detected by GB/T22374-2008 standards, as a result as follows:
The finish paint that can be seen that the present invention from the above-mentioned paint film calculation of measured data to finish paint made from the present embodiment has high hard
Degree, super abrasive and excellent adhesion strength.And construction appearance has the color sand granular sensation of tradition, with artistic effect,
Preferably beautify the environment.
Embodiment 2:
The anti-skidding finish paint of illusion-colour drawn grain of the present invention, including following components, by weight percentage for:
(1) mian paint includes:
128 epoxy resin 23.5%
Color sand particle 20%
Auxiliary agent:
Defoamer 1%
Levelling agent 2%
Dispersant 1%
Thixotropic agents:
Bentonite 5%
Modified aerosil 3%
Color stuffing:
Titanium dioxide 0.5%
Filler 29%
(2) curing agent:
Modified amine curing agent 15%
Take 128 resins in above-mentioned auxiliary agent add auxiliary agent it is well mixed after, add while stirring thixotropic agents bentonite and
Aerosil, titanium dioxide and filler, after disperseing 20 minutes at a high speed, below fineness 80um adds color sand particle stirring equal
It is even that the mian paint is made.
Modified amine curing agent is proportionally added into, paint film is prepared after stirring, paint film property presses GB/T22374-2008
Standard is detected, as a result as follows:
Test event | Standard requirement | Testing result |
Surface drying time | ≤6h | It is qualified |
Do solid work the time | ≤48h | It is qualified |
Pencil hardness | ≥2H | 4H |
Wear-resisting (750g/500r) | ≤30mg | 14mg |
I grade of shock resistance | Flawless, nothing comes off | It is qualified |
Resistance to marring | Nail is drawn without white trace | It is excellent |
Water resistance, 168h | It is non-foaming, do not fall off | It is qualified |
The solution of resistance to 20%NaOH, 72h | It is non-foaming, do not fall off | It is qualified |
Resistance to 10%H2SO4Solution, 48h | It is non-foaming, do not fall off | It is qualified |
VOC(g/L) | 60 | 28.3 |
Anti-skidding coefficient of friction | ≥0.5 | 1.03 |
The finish paint that can be seen that the present invention from the above-mentioned paint film calculation of measured data to finish paint made from the present embodiment has high hard
Degree, super abrasive, excellent adhesion strength.And construction appearance has the color sand granular sensation of tradition, with artistic effect, more preferably
Beautify the environment.
Embodiment 3:
The anti-skidding finish paint of illusion-colour drawn grain of the present invention, including following components, by weight percentage for:
(1) mian paint includes:
128 epoxy resin 28%
Color sand particle 15%
Thixotropic agents:
Bentonite 4%
Modified aerosil 1%
Auxiliary agent:
Defoamer 1.2%
Levelling agent 2.5%
Dispersant 1.0%
Color stuffing:
Titanium dioxide 0.5%
Filler 28.8%
(2) curing agent:
Modified amine curing agent 18%.
After 128 epoxy resin addition auxiliary agent in above-mentioned mian paint is well mixed, the swollen of thixotropic agents is added while stirring
The titanium dioxide and filler of profit soil and aerosil and color stuffing, after disperseing 20 minutes at a high speed, below fineness 80um, then add
Enter color sand particle and stir the mian paint is made;
Modified amine curing agent is added, finish paint is made after stirring, paint film is prepared with the finish paint, paint film property presses GB/
T22374-2008 standards are detected, as a result as follows:
Test event | Standard requirement | Testing result |
Surface drying time | ≤6h | It is qualified |
Do solid work the time | ≤48h | It is qualified |
Pencil hardness | ≥2H | 4H |
Wear-resisting (750g/500r) | ≤30mg | 16mg |
I grade of shock resistance | Flawless, nothing comes off | It is qualified |
Resistance to marring | Nail is drawn without white trace | It is excellent |
Water resistance, 168h | It is non-foaming, do not fall off | It is qualified |
The solution of resistance to 20%NaOH, 72h | It is non-foaming, do not fall off | It is qualified |
Resistance to 10%H2SO4Solution, 48h | It is non-foaming, do not fall off | It is qualified |
VOC(g/L) | 60 | 30.1 |
Anti-skidding coefficient of friction | ≥0.5 | 0.86 |
The finish paint that can be seen that the present invention from the above-mentioned paint film calculation of measured data to finish paint made from the present embodiment has high hard
Degree, super abrasive, excellent adhesion strength.And construction appearance has the color sand granular sensation of tradition, with artistic effect, more preferably
Beautify the environment.
The finish paint of the present invention improves the hardness of epoxy material and resisted by introducing the color sand particle of organic resin synthesis
Scratch resistant, while showing more rich colorful outward appearance;The uniform concaveconvex structure of coating surface, makes it have excellent friction system
Number, so as to reach more preferable skidproof effect.
The foregoing is only a preferred embodiment of the present invention, but protection scope of the present invention be not limited thereto,
Any one skilled in the art is in the technical scope of present disclosure, the change or replacement that can be readily occurred in,
It should all be included within the scope of the present invention.Therefore, protection scope of the present invention should be with the protection model of claims
Enclose and be defined.
Claims (8)
1. a kind of anti-skidding finish paint of illusion-colour drawn grain, it is characterised in that including following component by weight percentage:
2. the anti-skidding finish paint of illusion-colour drawn grain according to claim 1, it is characterised in that the epoxy resin uses bisphenol A-type
Epoxy resin.
3. the anti-skidding finish paint of illusion-colour drawn grain according to claim 1, it is characterised in that the curing agent uses modified fatty amine
Or modified polyether amine.
4. the anti-skidding finish paint of illusion-colour drawn grain according to claim 1, it is characterised in that the thixotropic agents using bentonite and
Modified aerosil, the consumption of each component is based on the percentage by weight of the total consumption of the anti-skidding finish paint of illusion-colour drawn grain, respectively:It is swollen
Profit soil 4~5%, modified aerosil 1~5%.
5. the anti-skidding finish paint of illusion-colour drawn grain according to claim 1, it is characterised in that the color sand particle is organic using import
Resin composite materials.
6. the anti-skidding finish paint of illusion-colour drawn grain according to any one of claim 1 to 5, it is characterised in that the auxiliary agent includes:Disappear
Infusion, levelling agent, dispersant, the consumption of each component is based on the percentage by weight of the total consumption of the anti-skidding finish paint of illusion-colour drawn grain, respectively:
Defoamer 0.8~1.5%, levelling agent 1.7~2.5%, dispersant 1%.
7. the anti-skidding finish paint of illusion-colour drawn grain according to any one of claim 1 to 5, it is characterised in that the color stuffing is used
Titanium dioxide and filler, the consumption of each component is based on the percentage by weight of the total consumption of the anti-skidding finish paint of illusion-colour drawn grain:Titanium dioxide 0.5~
1%, filler 14.5~29%.
8. a kind of preparation method of the anti-skidding finish paint of illusion-colour drawn grain, it is characterised in that for preparing any one of claim 1 to 7 institute
The anti-skidding finish paint of illusion-colour drawn grain stated, comprises the following steps:
The formula of the anti-skidding finish paint of illusion-colour drawn grain as described in any one of claim 1 to 5 takes each raw material;
After epoxy resin addition auxiliary agent is well mixed, thixotropic agents and color stuffing are added while stirring, it is scattered 20 minutes at a high speed
Afterwards, below fineness 80um, adds color sand particle and stirs mian paint is made;
Curing agent is added into above-mentioned mian paint, the anti-skidding finish paint of illusion-colour drawn grain is made after stirring.