CN109944091A - 一种柿漆漏板印染的方法及柿漆印花制品 - Google Patents

一种柿漆漏板印染的方法及柿漆印花制品 Download PDF

Info

Publication number
CN109944091A
CN109944091A CN201910299067.2A CN201910299067A CN109944091A CN 109944091 A CN109944091 A CN 109944091A CN 201910299067 A CN201910299067 A CN 201910299067A CN 109944091 A CN109944091 A CN 109944091A
Authority
CN
China
Prior art keywords
persimmon
printing
cloth
dyeing
paint
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910299067.2A
Other languages
English (en)
Inventor
唐锐
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Planting And Dyeing Blue Culture Creative Co Ltd
Original Assignee
Beijing Planting And Dyeing Blue Culture Creative Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Planting And Dyeing Blue Culture Creative Co Ltd filed Critical Beijing Planting And Dyeing Blue Culture Creative Co Ltd
Priority to CN201910299067.2A priority Critical patent/CN109944091A/zh
Publication of CN109944091A publication Critical patent/CN109944091A/zh
Pending legal-status Critical Current

Abstract

本发明提供一种柿漆漏板印染的方法,首先对布料进行单一颜色的柿漆印染,将布料柿染成浅褐色;其次配制印花糊料;再后将采用漏板印染的方式,对布料进行印花处理,得到经过两次柿漆印染具有精美花型的柿漆印染制品。本发明提供的方法采用两次媒染方法对布料进行处理,在两次媒染的过程中,只在第一次柿染纯色的基础布料的过程中使用柿漆,在第二次媒染过程中,直接在印花糊料中使用具有深色呈色性能的媒染剂,媒染剂能够与第一次使用的柿漆进行反应从而呈色,两次柿染,只使用到一次柿漆,减少了柿漆的使用量,降低了柿漆对布料的硬化影响,节约原料,本发明得到的的柿漆印染制品手感柔软、花型精美、安全性高。

Description

一种柿漆漏板印染的方法及柿漆印花制品
技术领域
本发明属于印染领域,具体涉及一种柿漆漏板印染的方法及得到的柿漆印花制品。
背景技术
印染是一种古老而现代的染色加工工艺。早在新石器时代,我们的祖先就开始使用磁铁矿粉对麻布进行染色;印染工艺经过了几千年的发现,染色技术不断提高,效率不断提升,印染的原料也得到不断的丰富。柿染是一种古老的印染方法,柿染采用柿漆进行印染。柿漆是选用未成熟而色青味涩的柿子,捣烂,置缸中加入适量清水,不时搅动,然后静置,过滤,得到无色的胶状液。柿染发色是利用柿漆中单宁在大气中发生氧化反应,在干燥以后被膜化形成不同的颜色。因柿漆中的单宁一旦与空气接触,便立即开始氧化,进而开始干燥着色,故柿染着色较强烈。由于柿漆的染色是氧化的过程,因此颜色会随着空气氧化的时间越久氧化程度会不断的加深,颜色有逐渐加深的趋势。但是柿染是一种古老的染色工艺,由于其需要需要原料来源并不广泛,处理困难,因此并没有得到广泛的应用,其柿染的工艺也相对传统。
柿染工艺目前多用于纯色物料的单一颜色印染或者在颜色偏浅的纯色底料上进行单色印花处理,目前柿染只能处理单一的色彩印染。并且目前柿染的过程是直接将柿漆与媒染剂进行混合,然后将印花糊料涂在空白处,然后将柿漆与媒染剂混合得到的混合液进行印花处理,干燥之后去除印花糊料,得到浅色底物的印花,而这一工艺不能在经过柿漆印染的布料上进行柿染印花处理,并不能得到具有花型图案的柿染印花布。此外目前的印花糊料的抱水性和渗水性并不适用于柿漆印染,存在柿漆印染过程中印花边界模糊不清,花纹达不到要求的问题。
发明内容
为了解决以上技术问题,本发明提供一种柿漆漏板印染的方法通过组合两种媒染剂,调整柿漆组分和印花糊料以及工艺,得到一种具有精美花型以及良好使用性能的柿漆印花产品。
本发明的目的是提供一种柿漆漏板印染的方法。
本发明的另一目的是提供一种上述方法得到的柿漆印花制品。
本发明提供的一种柿漆漏板印染的方法,包括以下步骤:
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:4.8-5.2的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:5-10的浴比充分浸泡在染液中染色,甩干、晾晒;
C1.将晒干的布料重新放入染液中重复步骤B1;
D1.将步骤C1染制过的布料投入到质量分数为0.8-1.2%的明矾溶液或质量分数为0.8-1.2%碳酸钠溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸亚铁、醋酸铁、硫酸铜或碳酸钾,加水,配制质量分数为2.5-3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:4.8-5.2的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,在纸板上涂刷生桐油,阴干,涂刷熟桐油,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
为了得到具有印花的柿漆印染制品,本发明首先对布料进行柿漆印染,得到具有浅色底色的柿漆纯色印染布料,再对布料进行柿漆印染的过程中,柿漆与水进行适当比例的混合,得到染液,将布料退浆之后,进行多次染色、甩干、晾晒,将柿漆进行稀释,然后进行反复的染色、甩干和晾晒,柿漆能够与布料纤维进行充分的接触,并且弱化了柿漆对布料的硬化,经过上述的方法进行柿漆染制得到的布料硬化程度较低,布料相对柔软,然后将处理过的布料投入到适当浓度的明矾溶液或者碳酸钠溶液中,明矾或碳酸钠中的铝粒子或者钠离子与柿漆发生金属络合反应,使得得到的布料呈现浅褐色;本发明提供的印花糊料包是黄豆粉、糯米粉和媒染剂以适当的比例进行混合得到,印花糊料中黄豆粉具有渗水性,糯米粉具有抱水性,上述的组分经过混合,得到的印花糊料中媒染剂与经过柿漆染制的布料中的柿漆充分融合,由于印花糊料中的媒染剂与柿漆经过金属络合反应之后,得到颜色相对较深的花型,因此能够在柿漆染制布料上印花;本发明提供的印花糊料通过黄豆粉、糯米粉以及媒染剂进行适当比例的混合,保证印花糊料中媒染剂与布料中的柿漆进行充分的接触,并且阻止媒染剂的外晕,提高花型印染的质量;本发明采用漏板印染的方式对柿漆染制布料进行印花处理,以纸板为印版的基材,在纸板上先涂刷生桐油附着力强能够在纸板上形成完整的保护膜,然后多次涂刷熟桐油,熟桐油能够快速的结膜,在生桐油表面形成具有较高的硬度和光泽度的膜层,避免印花糊料对印版的负面影响。
本发明提供的方法采用两次媒染方法对布料进行处理,在两次媒染的过程中,只在第一次柿染纯色的基础布料的过程中使用柿漆,在第二次媒染过程中,直接在印花糊料中使用具有深色呈色性能的媒染剂,媒染剂能够与第一次使用的柿漆进行反应从而呈色,两次柿染,只使用到一次柿漆,减少了柿漆的使用量,降低了柿漆对布料的硬化影响,节约原料,本发明得到的的柿漆印染制品手感柔软、花型精美、安全性高。
所述的柿漆漏板印染的方法,优选地,步骤(1)中,B1染色过程中还包括对布料进行持续揉搓15-25min,然后将布料取出,用木质棒槌捶打8-12min。由于柿漆与金属会有反应,因此本发明在进行柿漆印染的过程中,均采用不锈钢、塑料或者陶器作为容器,在布料的染制过程中,对布料进行揉搓和木棒捶打,促进柿漆与布料纤维之间的充分接触,提升染色的质量。
所述的柿漆漏板印染的方法,优选地,步骤(1)中,B1中晾晒为光照晾晒,晾晒的温度为15-40℃,时间为4h以上。
所述的柿漆漏板印染的方法,优选地,步骤(1)中,C1中,将晒干的布料重新放入到染液中重复步骤B1 6-9遍。由于柿漆会对布料产生硬化的影响,因此普通的柿染布料硬度较高,并不适用于作为衣物等面料,大大限制了柿染工艺的使用范围,本发明在将柿漆进行稀释,然后对布料进行多次的浸染,布料与稀释过的染液进行充分的接触,染液中的柿漆有效成分与布料纤维之间充分结合,并且经过多的揉搓捶打,布料的硬化程度会得到有效的改善。
所述的柿漆漏板印染的方法,优选地,步骤(1)中,D1中,媒染的时间为15-25min。
所述的柿漆漏板印染的方法,优选地,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的醋酸铁水溶液。本发明的媒染剂可以是质量分数为2.5-3%的醋酸铁水溶液,醋酸铁水溶液中的铁离子能够与柿漆发生金属络合反应,在浅褐色的底色上呈现黑色,从而呈现柿染花型。
所述的柿漆漏板印染的方法,优选地,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的硫酸铜水溶液。本发明的媒染剂可以是质量分数为2.5-3%的硫酸铜水溶液,硫酸铜水溶液中的铜离子能够与柿漆发生金属络合反应,在浅褐色的底色上呈现深褐色,从而呈现柿染花型。
所述的柿漆漏板印染的方法,优选地,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的碳酸钾水溶液。本发明的媒染剂可以是质量分数为2.5-3%的碳酸钾水溶液,碳酸钾能够与柿漆发生金属络合反应,在浅褐色的底色上呈现红褐色,从而呈现柿染花型。
所述的柿漆漏板印染的方法,优选地,步骤(3)中,A3中,所述纸板的厚度为0.2-0.6mm,所述熟桐油涂刷的次数为2-3次。本发明采用经过生桐油和熟桐油涂刷过的纸板作为漏板进行花型的印制,在柿染印制花型的过程中,印版的厚度决定了印花糊料的用量和厚度,从而影响印染的品质,本发明提供的印版厚度下,印花糊料中的媒染剂能够渗透至基材,与基材布料中的柿漆进行充分的反应,同时,印花糊料中的抱水性成分又能组织媒染剂相花型的周边扩散,避免晕染。多次涂刷熟桐油也能够保证在印版表面形成光滑、防水的膜层,避免印花糊料对印版的影响,保证印花的精确度。
本发明的有益效果为:
本发明提供一种柿漆漏板印染的方法,首先对布料进行单一颜色的柿漆印染,将布料柿染成浅褐色;其次配制印花糊料;再后将采用漏板印染的方式,对布料进行印花处理,得到经过两次柿漆印染具有精美花型的柿漆印染制品。本发明提供对布料进行初次纯色柿漆印染的过程中,将柿漆进行加水稀释,进行多次的浸染、捶打,保证布料的柔软度,然后进行浅色媒染剂媒染,浅色的媒染剂与柿漆进行金属络合反应,得到纯色的浅色柿染布料;本发明提供的印花糊料包括糯米粉、黄豆粉和深色的媒染剂,其中糯米粉具有良好的抱水性,避免印花糊料中的水分向周向扩散,保证印花的精确度,黄豆粉具有良好的渗水性,保证印花糊料中媒染剂能够随水进行垂直方向的扩散,与经过初步柿染的布料进行充分的接触,印花糊料中的深色媒染剂与经过柿染布料中的柿漆发生金属络合反应,在浅色柿染布料上呈现深色花型。本发明提供的方法采用两次媒染方法对布料进行处理,在两次媒染的过程中,只在第一次柿染纯色的基础布料的过程中使用柿漆,在第二次媒染过程中,直接在印花糊料中使用具有深色呈色性能的媒染剂,媒染剂能够与第一次使用的柿漆进行反应从而呈色,两次柿染,只使用到一次柿漆,减少了柿漆的使用量,降低了柿漆对布料的硬化影响,节约原料,本发明得到的的柿漆印染制品手感柔软、花型精美、安全性高。
具体实施方式
为使本发明的目的、技术方案和优点更加清楚,下面将对本发明的技术方案进行详细的描述。显然,所描述的实施例仅仅是本发明一部分实施例,而不是全部的实施例。基于本发明中的实施例,本领域普通技术人员在没有做出创造性劳动的前提下所得到的所有其它实施方式,都属于本发明所保护的范围。
实施例1
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:4.8的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:5的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓15min然后将布料取出,用木质棒槌捶打8min,甩干、在阳光下晾晒,晾晒的温度为30-40℃,晾晒4h;
C1.将晒干的布料重新放入染液中重复步骤B1 6遍;
D1.将步骤C1染制过的布料投入到质量分数为0.8%的明矾溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸亚铁,加水,配制质量分数为2.5%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:4.8的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.2mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油2次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例2
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5.2的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓25min然后将布料取出,用木质棒槌捶打12min,甩干、在阳光下晾晒,晾晒的温度为30-35℃,晾晒5h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1.2%的明矾溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸亚铁,加水,配制质量分数为3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.6mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例3
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为15-20℃,晾晒6h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1%的明矾溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取醋酸铁,加水,配制质量分数为3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5.2的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例4
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为15-20℃,晾晒6h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为0.8%的碳酸钠溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取醋酸铁,加水,配制质量分数为2.5%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例5
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为30-35℃,晾晒5h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1%的碳酸钠溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸铜,加水,配制质量分数为3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例6
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为30-35℃,晾晒5h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1.2%的碳酸钠溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸铜,加水,配制质量分数为2.5%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例7
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为30-35℃,晾晒5h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1%的明矾溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取碳酸钾,加水,配制质量分数为3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
实施例8
一种柿漆漏板印染的方法,包括以下步骤;
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:5的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:10的浴比充分浸泡在染液中染色,在染色过程中对布料进行持续揉搓20min然后将布料取出,用木质棒槌捶打10min,甩干、在阳光下晾晒,晾晒的温度为30-35℃,晾晒5h;
C1.将晒干的布料重新放入染液中重复步骤B1 9遍;
D1.将步骤C1染制过的布料投入到质量分数为1%的明矾溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取碳酸钾,加水,配制质量分数为2.5%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:5的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,所述纸板的厚度为0.5mm,在纸板上涂刷生桐油,阴干,涂刷熟桐油3次,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
试验例
试验例1
实施例2得到的印花糊料。
对比例1
将黄豆粉与3%的硫酸亚铁溶液按照重量比3:5的比例进行混合,得到印花糊料1。
对比例2
将糯米粉与3%硫酸亚铁溶液按重量比3:5的比例进行混合,得到印花糊料2。
检测试验例1、对比例1和对比例2得到的印花糊料的各项性能,结果见表1。
表1检测结果
性能 对比例1 对比例2 试验例1
粘度(Pa.s) 15000 40000 25000
粘度PVI 0.6 0.3 0.5
抱水性 0.3cm/30m 0.1cm/30m 0.2cm/30m
得色量
手感
水洗色牢度 3-4级 3级 3-4级
印制效果
从表1的结果可以看出,本发明提供的印花糊料具有适宜的粘度,本发明采用漏板印染的方式进行,在印染的过程中,色浆在筛网版上受到刮刀给予的压力与剪切力,色浆所述的剪切力小,要求印花糊料具有良好的流变性能,同时要求印花糊料具有一定的粘度,在结束印染之后,印花糊料不至于飞浆。本发明提供的印花糊料粘度适中,配合漏板印染,得到的制品手感良好,得色量适中,抱水量适中,水洗色牢度较高,印制效果优秀。
以上所述,仅为本发明的具体实施方式,但本发明的保护范围并不局限于此,任何熟悉本技术领域的技术人员在本发明揭露的技术范围内,可轻易想到变化或替换,都应涵盖在本发明的保护范围之内。因此,本发明的保护范围应以所述权利要求的保护范围为准。

Claims (10)

1.一种柿漆漏板印染的方法,其特征在于,包括以下步骤:
(1)柿漆染制布料:
A1.将柿漆与水按照体积比为1:4.8-5.2的比例进行混合,搅拌均匀,得到染液;
B1.将布料退浆,按照1:5-10的浴比充分浸泡在染液中染色,甩干、晾晒;
C1.将晒干的布料重新放入染液中重复步骤B1;
D1.将步骤C1染制过的布料投入到质量分数为0.8-1.2%的明矾溶液或质量分数为0.8-1.2%碳酸钠溶液中媒染,甩干、晾干,得到染制布料;
(2)配制印花糊料:
A2.取硫酸亚铁,加水,配制质量分数为2.5-3%的媒染剂溶液;
B2.将黄豆粉、糯米粉与步骤A2得到的媒染剂溶液按照重量比为2:1:4.8-5.2的比例混合,得到印花糊料;
(3)印染花型:
A3.将需要的花型以镂空的方式雕刻在纸板上,在纸板上涂刷生桐油,阴干,涂刷熟桐油,阴干,得到印版;
B3.将印版覆盖在步骤(1)得到的染制布料上,将步骤(2)配置好的印花糊料通过印版将图案印制到染制布料上,干燥;
C3.去除印花上的印花糊料,将处理过的布料放入到清水中浸泡、洗涤、晾干,得到柿漆漏板印染制品。
2.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(1)中,B1染色过程中还包括对布料进行持续揉搓15-25min,然后将布料取出,用木质棒槌捶打8-12min。
3.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(1)中,B1中晾晒为光照晾晒,晾晒的温度为15-40℃,时间为4h以上。
4.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(1)中,C1中,将晒干的布料重新放入到染液中重复步骤B1 6-9遍。
5.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(1)中,D1中,媒染的时间为15-25min。
6.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的醋酸铁水溶液。
7.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的硫酸铜水溶液。
8.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(2)中,A2中所述媒染剂溶液为质量分数为2.5-3%的碳酸钾水溶液。
9.根据权利要求1所述的柿漆漏板印染的方法,其特征在于,步骤(3)中,A3中,所述纸板的厚度为0.2-0.6mm,所述熟桐油涂刷的次数为2-3次。
10.权利要求1-9任一所述的方法得到的柿漆印花制品。
CN201910299067.2A 2019-04-15 2019-04-15 一种柿漆漏板印染的方法及柿漆印花制品 Pending CN109944091A (zh)