CN108440975A - A kind of chromatic bitumen mixture - Google Patents
A kind of chromatic bitumen mixture Download PDFInfo
- Publication number
- CN108440975A CN108440975A CN201810278032.6A CN201810278032A CN108440975A CN 108440975 A CN108440975 A CN 108440975A CN 201810278032 A CN201810278032 A CN 201810278032A CN 108440975 A CN108440975 A CN 108440975A
- Authority
- CN
- China
- Prior art keywords
- parts
- petropols
- pigment
- added
- bitumen mixture
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of chromatic bitumen mixtures, are made of the raw material of following parts by weight:15 20 parts of C5 Petropols, 20 30 parts of C9 Petropols, 30 35 parts of base oil, 38 parts of styrene butadiene rubber powder, 5 12 parts of inorganic pigment, 30 40 parts of miberal powder, 25 35 parts of mountain flour.The present invention can produce the chromatic bitumen mixture of various colors, improve vision, can be widely used in the different places such as street, pavement and landscape road, can not only meet the needs of various places, while can also beautify the environment.The present invention realizes the color asphalt product for being prepared have excellent performance at lower cost by being formulated global design.
Description
Technical field
The present invention relates to technical field of road engineering, more particularly to a kind of chromatic bitumen mixture.
Background technology
Elasticity of the Colorful Asphalt Pavement with asphalt concrete is strong, damping strong and is easy to clean the formedness such as flushing
Can be outer, the monotonicity of plain asphalt road surface black is further improved, can be collocated with each other, coordinate with the building of surrounding, landscape, have
Apparent Landscape benefit.In addition, color asphalt increasingly obtains the organization and management effect of traffic the attention of people.Different colours
Bituminous paving, the recognition effect of driver can be improved, and the attention of driver can also be made more to concentrate, to play
Induce wagon flow, safe driving, the effect for making traffic administration intuitively change.It, can be with such as in the multiple location of Urban Road Traffic Accidents
Driver is intuitively reminded note that driving a vehicle with caution, to a certain extent than vertical traffic sign in making red or yellow road surface
And stroke markings are more preferable on track.
But the performance of existing color asphalt is still to be improved.
Invention content
In order to make up the defect of prior art, the present invention provides a kind of chromatic bitumen mixture.
The technical problems to be solved by the invention are achieved by the following technical programs:
A kind of chromatic bitumen mixture is made of the raw material of following parts by weight:15-20 parts of C5 Petropols, C9 oil trees
20-30 parts of fat, 30-35 parts of base oil, 3-8 parts of styrene butadiene rubber powder, 5-12 parts of inorganic pigment, 30-40 parts of miberal powder, mountain flour 25-35
Part.
Further, inorganic pigment be iron oxide red pigment, chrome green pigment, iron green pigment, titanium dioxide pigment, in chrome yellow extremely
Few one kind.
Further, preparation method includes the following steps:(1)Base oil is added according to the parts by weight, is heated to
Under the conditions of 165-190 DEG C, styrene butadiene rubber powder stirring melting is added, C5 Petropols, C9 Petropols are added after being completely dissolved, most
After inorganic pigment is added, after being uniformly mixed, that is, prepare color asphalt;(2)By step(1)The color asphalt of gained heats
To 92-100 DEG C, it is added directly into mixing in cylinder for asphalt mixing plant, then with miberal powder, mountain flour mix and stir obtained
Product.
The present invention has the advantages that:
The present invention can produce the chromatic bitumen mixture of various colors, improve vision, can be widely used in street, people
The different places such as trade and landscape road can not only meet the needs of various places, while can also beautify the environment.
The present invention realizes the color asphalt production for being prepared have excellent performance at lower cost by being formulated global design
Product.
Specific implementation mode
With reference to embodiment, the present invention will be described in detail, and embodiment is only the preferred embodiment of the present invention,
It is not limitation of the invention.
Embodiment 1
A kind of chromatic bitumen mixture is made of the raw material of following parts by weight:18 parts of C5 Petropols, C9 Petropols 25
Part, 32 parts of base oil, 5 parts of styrene butadiene rubber powder, 8 parts of inorganic pigment, 35 parts of miberal powder, 30 parts of mountain flour.
Wherein, inorganic pigment is iron oxide red pigment.
Preparation method includes the following steps:(1)Base oil is added according to the parts by weight, is heated to 165-190 DEG C
Under the conditions of, styrene butadiene rubber powder stirring melting is added, C5 Petropols, C9 Petropols are added after being completely dissolved, are eventually adding nothing
Machine pigment after being uniformly mixed, that is, prepares color asphalt;(2)By step(1)The color asphalt of gained is heated to 92-100
DEG C, it is added directly into mixing in cylinder for asphalt mixing plant, then carries out mixing and stirring obtained product with miberal powder, mountain flour.
Embodiment 2
A kind of chromatic bitumen mixture is made of the raw material of following parts by weight:15 parts of C5 Petropols, C9 Petropols 20
Part, 30 parts of base oil, 3 parts of styrene butadiene rubber powder, 5 parts of inorganic pigment, 30 parts of miberal powder, 25 parts of mountain flour.
Wherein, inorganic pigment is chrome green pigment.
Preparation method includes the following steps:(1)Base oil is added according to the parts by weight, is heated to 165-190 DEG C
Under the conditions of, styrene butadiene rubber powder stirring melting is added, C5 Petropols, C9 Petropols are added after being completely dissolved, are eventually adding nothing
Machine pigment after being uniformly mixed, that is, prepares color asphalt;(2)By step(1)The color asphalt of gained is heated to 92-100
DEG C, it is added directly into mixing in cylinder for asphalt mixing plant, then carries out mixing and stirring obtained product with miberal powder, mountain flour.
Embodiment 3
A kind of chromatic bitumen mixture is made of the raw material of following parts by weight:20 parts of C5 Petropols, C9 Petropols 30
Part, 35 parts of base oil, 8 parts of styrene butadiene rubber powder, 12 parts of inorganic pigment, 40 parts of miberal powder, 35 parts of mountain flour.
Wherein, inorganic pigment is at least one in iron oxide red pigment, chrome green pigment, iron green pigment, titanium dioxide pigment, chrome yellow
Kind.
Preparation method includes the following steps:(1)Base oil is added according to the parts by weight, is heated to 165-190 DEG C
Under the conditions of, styrene butadiene rubber powder stirring melting is added, C5 Petropols, C9 Petropols are added after being completely dissolved, are eventually adding nothing
Machine pigment after being uniformly mixed, that is, prepares color asphalt;(2)By step(1)The color asphalt of gained is heated to 92-100
DEG C, it is added directly into mixing in cylinder for asphalt mixing plant, then carries out mixing and stirring obtained product with miberal powder, mountain flour.
Embodiments of the present invention above described embodiment only expresses, the description thereof is more specific and detailed, but can not
Therefore it is interpreted as the limitation to the scope of the claims of the present invention, as long as skill obtained in the form of equivalent substitutions or equivalent transformations
Art scheme should all be fallen within the scope and spirit of the invention.
Claims (3)
1. a kind of chromatic bitumen mixture, which is characterized in that it is made of the raw material of following parts by weight:C5 Petropols 15-
20 parts, 20-30 parts of C9 Petropols, 30-35 parts of base oil, 3-8 parts of styrene butadiene rubber powder, 5-12 parts of inorganic pigment, miberal powder 30-40
Part, 25-35 parts of mountain flour.
2. chromatic bitumen mixture as described in claim 1, which is characterized in that inorganic pigment be iron oxide red pigment, chrome green pigment,
At least one of iron green pigment, titanium dioxide pigment, chrome yellow.
3. chromatic bitumen mixture as described in claim 1, which is characterized in that preparation method includes the following steps:(1)According to
Base oil is added in the parts by weight, is heated under the conditions of 165-190 DEG C, and styrene butadiene rubber powder stirring melting is added, is completely dissolved
C5 Petropols, C9 Petropols are added afterwards, is eventually adding inorganic pigment, after being uniformly mixed, that is, prepares color asphalt;
(2)By step(1)The color asphalt of gained is heated to 92-100 DEG C, and be added directly into asphalt mixing plant mixes cylinder
In, then carry out mixing and stirring obtained product with miberal powder, mountain flour.