CN106884535A - A kind of construction technology of imitative stone material Self-leveling waterproof mortar - Google Patents
A kind of construction technology of imitative stone material Self-leveling waterproof mortar Download PDFInfo
- Publication number
- CN106884535A CN106884535A CN201710041173.1A CN201710041173A CN106884535A CN 106884535 A CN106884535 A CN 106884535A CN 201710041173 A CN201710041173 A CN 201710041173A CN 106884535 A CN106884535 A CN 106884535A
- Authority
- CN
- China
- Prior art keywords
- leveling
- self
- water
- construction
- mortar
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of construction technology of imitative stone material Self-leveling waterproof mortar, comprise the following steps:Equipment prepares with instrument, base treatment, brushing interfacial agents, dispensing, cast, maintenance, expansion joint treatment, speed of application can be greatly speeded up using imitative stone material Self-leveling waterproof mortar, reduce labour intensity, improve using effect, for basic unit to be levelling and once visited place face, dusting ground and unqualified ground repairing of constructing, at the same time as epoxy floor or can require that foundation base intension screed-coat high is used as PVC coiled materials, basic unit's alignment material of composite floor board.
Description
Technical field
The present invention relates to building material technical field, specially a kind of construction technology of imitative stone material Self-leveling waterproof mortar.
Background technology
Waterproof mortar is called cationic chloroprene latex water-proof and anti-corrosive material.Cationic chloroprene latex is a kind of high polymer point
The modified based high molecular water-tight corrosion-proof system of son.By being introduced into mouthful epoxy resin modified latex acceding state neoprene latex and poly-
The high polymer latex that acrylate, synthetic rubber, various emulsifying agents, modified latex etc. are constituted.Add base-material and appropriate chemistry
Auxiliary agent and inserts, through plasticating, knead, the macromolecule water-proof and anti-corrosive material that the operation such as calendering is added.From imported material
With domestic high-quality auxiliary material, according to the quality product of national sector standard highest ranking written instructions production, national Research of Comfortable House is pushed away
Recommend product.Long lifespan, easy construction, long period of soaking in water the life-span more than 50 years.
Waterproof mortar has a good weatherability, durability, impervious, density and high bonding force and extremely strong
Water-tight corrosion-proof effect.It is resistant to soda manufacture medium, urea, ammonium nitrate, seawater hydrochloric acid and acid-base property salt corrosion.It is with sand light water
Mud and special cement are configured to cement mortar, by reconcile cement mortar cast or spray, by hand smear method in concrete
And surface forms firm water-tight corrosion-proof screed, belong to strong and unyielding property water-proof and anti-corrosive material.With cement, sand mixes can change mortar
Property, can be used for treatment and the underground project waterproof layer on building wall and ground.
Gravity flow flat ground material is typically as different decorative floors (such as carpet, PVC floor, epoxide terrace, polyurethane
Level ground, timber floor etc.) bed course, be a part for whole ground screed systems, can be used for large area, have to flatness strictly will
The ground construction asked, such as use requirement industrial premises higher, supermarket, warehouse, exhibition room, parking lot, library, airport, station
, ground renovation repairing levelling etc. public, civilian hall floor and ground waterproof.The characteristics of using gravity flow flat ground material, can be to passing
The speed of application of system mortar is expired, and the big problem of construction labour intensity is improved.
The content of the invention
It is an object of the invention to provide one kind using imitative stone material gravity flowing levelling mortar, speed of application can be greatly speeded up, reduced
Labour intensity, using effect is improved, for basic unit to be levelling and once visited place face, dusting ground and unqualified ground repairing of constructing, can
As PVC coiled materials, basic unit's alignment material of composite floor board, at the same time as epoxy floor or require that foundation base intension is high
Screed-coat is used, to solve the problems, such as to be proposed in above-mentioned background technology.
To achieve the above object, the present invention provides following technical scheme:A kind of construction of imitative stone material Self-leveling waterproof mortar
Technique, it is characterised in that:Comprise the following steps:
(1)Equipment and instrument prepare, according to common process requirement prepare 300 revs/min slow-speed of revolution agitator, ground sander,
Air compressor, vacuum cleaner, electric slicer, level meter, ground pull strength somascope, fluidity tester, painting brush
Or roller, steel ladle, special spikes, deflation roller, glue bucket, tooth form trowel, cylinder rain boots high, nail footwear;
(2)Base treatment, basic unit must it is clean, solid, smooth, can load-bearing, without greasy dirt, loose matter;Basic unit's compression strength exists
Draw and dial intensity not less than 1.5MPa in more than 20MPa, the surface of basic unit;If original basic unit's concrete ground intensity is too low, surface has floating
Slurry or dusting are serious, then must polish, until exposing solid surface;The cement mortar dust and discarded object of polishing are cleared up, is used first
Broom is cleaned one time, then is cleaned with dust catcher dust suction and with water, if there is oil stain on basal plane, chemical treatment can be used, so
Rinsed with clean water afterwards;If there is seepage in basic unit, water-proofing treatment must be in advance carried out;Basal plane is newly-laid concrete or mortar, then need
Self-leveling construction can be carried out after intensity reaches more than 20MPa, age at least 4 weeks;
(3)Brushing interfacial agents, paint interfacial agents on basal plane, day heated drying or basal plane porous water-absorbing are very strong, then should brush 1-3
Being rinsed with clean water before hour allows basal plane fully to soak, and ensures that basal plane, will with painting brush or roller without bright water before brush interfacial agents
Self-leveling interfacial agents are applied on concrete surface, brush secondary, are constructed using crossing method, and ground floor can apply the after drying
Two layers, self-leveling material could be poured into a mould after waiting last time interfacial agents dry;
(4)When dispensing, small area or lattice are constructed, it is stirred in bucket with minitype electric mixer, often stirs and once use
A complete whole bag;During large-area construction, stirred with special-purpose stirring machine, the method pumped with mortar is constructed;The slurry mixed should be 30
It is finished in minute, slurry supply is timely, it is ensured that the continuity of the whole scope of operation;
(5)Cast, working region is allowed slightly to divulge information, but door and window should be closed, and be must assure that before cast on basal plane without water,
Indoor and surface temperature should be higher than that 10 DEG C during construction and in construction one week after;, it is necessary to according to the scope of operation before gravity flowing levelling mortar construction
Width and field condition set construction joint, and cement self-leveling operation side width is no more than 6~8 meters;The gravity flow that will be stirred
Flat mortar falls on basal plane, uniformly spreads out, and is struck off with special tooth mouthful scraper plate, then with mace reciprocating rolling with profit exhaust and
Elimination connects stubble, and treating that it is smeared from putting down, once must reach required thickness, after surface condenses, can not smear again;The strip gravity flow of cast
Flat material should reach design thickness, if Self-leveling construction thickness design is less than 3mm, need to use special tooth mouthful scraper plate to be subject to
Control;The auto-flowing floor that the rapid mace rolling of drift bolt footwear was poured into a mould is to discharge the air brought into during stirring, it is to avoid bubble,
The interface discrepancy in elevation between pitted skin and bar and bar;Used instrument and equipment should be cleaned with water in time;
(6)Maintenance, is not usually required to maintenance, if environment temperature is very high, sun direct projection, be air-dried situation if need to be conserved,
Plastic foil is covered on and conserved two days in the gravity flow flat surface of firmization;
(7)Expansion joint is processed, after auto-flowing floor construction terminates 24 hours, can be with cutting machine in substrate concrete structure
The expansion joint of 3mm is cut out at expansion joint, the expansion joint of well cutting is cleaned out, sealed with elastic sealant and filled.
Preferably, step(2)The crack of substrate surface will pick and dig into " V " type when middle basic unit has the seepage to carry out water-proofing treatment
Groove, and it is smooth with gravity flowing levelling mortar repairing, and pit, hole must also be repaired smooth with gravity flowing levelling mortar.
Preferably, step(4)Middle match ratio is that every 25 kilograms of powders add 5.5 liters of clear water, it is impossible to arbitrarily increase water, will
Load weighted water is placed in clean agitator, starts electric mixer, and whole bag self-leveling material, continuous uniform ground are added slowly
Stirring 3 ± 1 minutes, to the uniform slurry without caking is formed, after standing 3-5 minutes, is stirred for 1 minute, and check slurry
Mobile performance, qualified to can be used, mixing time can not be long, in order to avoid it is mixed into excessive air.
Preferably, in construction technology work progress, U.S. line paper 5-7cm of stickup wide is complete in floor construction on skirting board
Afterwards, unnecessary U.S. line paper is removed with blade.
Compared with prior art, the beneficial effects of the invention are as follows:Can be greatly speeded up using imitative stone material Self-leveling waterproof mortar
Speed of application, reduces labour intensity, improves using effect, for basic unit to be levelling and once visited place face, dusting ground and construction do not conform to
Lattice ground is repaired, can be as PVC coiled materials, basic unit's alignment material of composite floor board, at the same time as epoxy floor or will
The screed-coat for asking foundation base intension high is used.It possesses high fluidity energy, can Self-leveling, good stability, condense before be not layered
Isolation, excreting water phenomenon, early strong, high-strength, later strength not retraction, adhesion strength is high, good toughness, and durability is high, and volume stability is low
Shrink, cracking resistance, waterproof, protection against the tide, easy to operate, quick construction can carry out large area jointless construction, green ring in a short time
Protect, it is nontoxic, pollution-free, "dead", many advantages, such as harmless.
Specific embodiment
The technical scheme in the embodiment of the present invention will be clearly and completely described below, it is clear that described implementation
Example is only a part of embodiment of the invention, rather than whole embodiments.Based on the embodiment in the present invention, this area is common
The every other embodiment that technical staff is obtained under the premise of creative work is not made, belongs to the model of present invention protection
Enclose.
The present invention provides a kind of technical scheme:A kind of construction technology of imitative stone material Self-leveling waterproof mortar, including following step
Suddenly:
(1)Equipment and instrument prepare, according to common process requirement prepare 300 revs/min slow-speed of revolution agitator, ground sander,
Air compressor, vacuum cleaner, electric slicer, level meter, ground pull strength somascope, fluidity tester, painting brush
Or roller, steel ladle, special spikes, deflation roller, glue bucket, tooth form trowel, cylinder rain boots high, nail footwear;
(2)Base treatment, basic unit must it is clean, solid, smooth, can load-bearing, without greasy dirt, loose matter;Basic unit's compression strength exists
Draw and dial intensity not less than 1.5MPa in more than 20MPa, the surface of basic unit;If original basic unit's concrete ground intensity is too low, surface has floating
Slurry or dusting are serious, then must polish, until exposing solid surface;The cement mortar dust and discarded object of polishing are cleared up, is used first
Broom is cleaned one time, then is cleaned with dust catcher dust suction and with water, if there is oil stain on basal plane, chemical treatment can be used, so
Rinsed with clean water afterwards;If there is seepage in basic unit, water-proofing treatment must be in advance carried out;Basal plane is newly-laid concrete or mortar, then need
Self-leveling construction can be carried out after intensity reaches more than 20MPa, age at least 4 weeks;
(3)Brushing interfacial agents, paint interfacial agents on basal plane, day heated drying or basal plane porous water-absorbing are very strong, then should brush 1-3
Being rinsed with clean water before hour allows basal plane fully to soak, and ensures that basal plane, will with painting brush or roller without bright water before brush interfacial agents
Self-leveling interfacial agents are applied on concrete surface, brush secondary, are constructed using crossing method, and ground floor can apply the after drying
Two layers, self-leveling material could be poured into a mould after waiting last time interfacial agents dry;
(4)When dispensing, small area or lattice are constructed, it is stirred in bucket with minitype electric mixer, often stirs and once use
A complete whole bag;During large-area construction, stirred with special-purpose stirring machine, the method pumped with mortar is constructed;The slurry mixed should be 30
It is finished in minute, slurry supply is timely, it is ensured that the continuity of the whole scope of operation;
(5)Cast, working region is allowed slightly to divulge information, but door and window should be closed, and be must assure that before cast on basal plane without water,
Indoor and surface temperature should be higher than that 10 DEG C during construction and in construction one week after;, it is necessary to according to the scope of operation before gravity flowing levelling mortar construction
Width and field condition set construction joint, and cement self-leveling operation side width is no more than 6~8 meters;The gravity flow that will be stirred
Flat mortar falls on basal plane, uniformly spreads out, and is struck off with special tooth mouthful scraper plate, then with mace reciprocating rolling with profit exhaust and
Elimination connects stubble, and treating that it is smeared from putting down, once must reach required thickness, after surface condenses, can not smear again;The strip gravity flow of cast
Flat material should reach design thickness, if Self-leveling construction thickness design is less than 3mm, need to use special tooth mouthful scraper plate to be subject to
Control;The auto-flowing floor that the rapid mace rolling of drift bolt footwear was poured into a mould is to discharge the air brought into during stirring, it is to avoid bubble,
The interface discrepancy in elevation between pitted skin and bar and bar;Used instrument and equipment should be cleaned with water in time;
(6)Maintenance, is not usually required to maintenance, if environment temperature is very high, sun direct projection, be air-dried situation if need to be conserved,
Plastic foil is covered on and conserved two days in the gravity flow flat surface of firmization;
(7)Expansion joint is processed, after auto-flowing floor construction terminates 24 hours, can be with cutting machine in substrate concrete structure
The expansion joint of 3mm is cut out at expansion joint, the expansion joint of well cutting is cleaned out, sealed with elastic sealant and filled.
Wherein step(2)The crack of substrate surface will pick and dig into " V " type groove when middle basic unit has the seepage to carry out water-proofing treatment,
And it is smooth with gravity flowing levelling mortar repairing, pit, hole must also be repaired smooth with gravity flowing levelling mortar.Step(4)Middle match ratio is
Every 25 kilograms of powders add 5.5 liters of clear water, it is impossible to arbitrarily increase water, load weighted water is placed in clean agitator, open
Dynamic electric mixer, adds whole bag self-leveling material slowly, and continuous uniform ground stirring 3 ± 1 minutes is starched to formation is uniform without caking
Untill body, after standing 3-5 minutes, it is stirred for 1 minute, and checks the mobile performance of slurry, qualified to can be used, mixing time is not
Can be long, in order to avoid it is mixed into excessive air.Associated technical parameters after construction are as shown in Table 1:
Table one
Simultaneously in construction technology work progress, 5-7cm U.S. line paper wide is pasted on skirting board, after floor construction is complete,
Unnecessary U.S. line paper is removed with blade.Speed of application can be greatly speeded up using imitative stone material Self-leveling waterproof mortar, work is reduced
Intensity, using effect is improved, for basic unit to be levelling and once visited place face, dusting ground and unqualified ground repairing of constructing, can conduct
Basic unit's alignment material of PVC coiled materials, composite floor board, at the same time as epoxy floor or requires high levelling of foundation base intension
Layer is used.It possesses high fluidity energy, can Self-leveling, there is no laminated segregation, excreting water phenomenon before condensing in good stability, it is early by force,
It is high-strength, later strength not retraction, adhesion strength is high, good toughness, and durability is high, volume stability, lower shrinkage, cracking resistance, waterproof, anti-
Tide, easy to operate, quick construction can carry out large area jointless construction in a short time, environmental protection, it is nontoxic, without dirt
Dye, it is "dead", many advantages, such as harmless.
Because the imitative stone material Self-leveling waterproof mortar is the material of cement base, the energy of resistant to dust and the liquid pollution on its surface
Power and other cement-based materials are similar, in having the environment compared with high-cleanness requirement, recommend using appropriate surface treatment and ground
Protect in face.Ground can be protected in the agent of surface spraying surface-closed, and increase surface colour after gravity flow plane layer is fully cured
Color gorgeous property and durability degree.Associated materials consumption is as shown in Table 2:
Base Smoothness | Levelling is thick(mm) | Proportioning reference(Ratio of water to material) | Levelling pass | |
Elementary errors basal plane | 2 | 3 | 0.22~0.25 | 1 |
General basal plane | 3 | 4.5 | 0.18~0.22 | 1 |
The standard total space, one levelling | 6 | 9 | 0.25~0.30 | 1-2 |
Interfacial agents | 1 | 0.2-0.3kg/m 2 (one time) | — | 1 |
Table two
Although an embodiment of the present invention has been shown and described, for the ordinary skill in the art, it is possible to understand that
These embodiments can be carried out with various changes, modification, replacement without departing from the principles and spirit of the present invention and become
Type, the scope of the present invention be defined by the appended.
Claims (4)
1. a kind of construction technology of imitative stone material Self-leveling waterproof mortar, it is characterised in that:Comprise the following steps:
Equipment prepares with instrument, and 300 revs/min of slow-speed of revolution agitator, ground sander, sky are prepared according to common process requirement
Air compressor, vacuum cleaner, electric slicer, level meter, ground pull strength somascope, fluidity tester, painting brush or
Roller, steel ladle, special spikes, deflation roller, glue bucket, tooth form trowel, cylinder rain boots high, nail footwear;
Base treatment, basic unit must it is clean, solid, smooth, can load-bearing, without greasy dirt, loose matter;Basic unit's compression strength is in 20MPa
More than, the surface of basic unit is drawn and dials intensity not less than 1.5MPa;If original basic unit's concrete ground intensity is too low, there is laitance on surface or
Dusting is serious, then must polish, until exposing solid surface;The cement mortar dust and discarded object of polishing are cleared up, broom is used first
Clean one time, then cleaned with dust catcher dust suction and with water, if there is oil stain on basal plane, chemical treatment, Ran Houyong can be used
Clean water is rinsed;If there is seepage in basic unit, water-proofing treatment must be in advance carried out;Basal plane is newly-laid concrete or mortar, then need to be strong
Degree can carry out Self-leveling construction after reaching more than 20MPa, age at least 4 weeks;
Brushing interfacial agents, paint interfacial agents on basal plane, day heated drying or basal plane porous water-absorbing are very strong, then should be small in brushing 1-3
When before rinsed with clean water and allow basal plane fully to soak, basal plane is ensured before brush interfacial agents without bright water, will be from painting brush or roller
Levelling interfacial agents are applied on concrete surface, and brushing is secondary, are constructed using crossing method, and ground floor can apply second after drying
Layer, self-leveling material could be poured into a mould after waiting last time interfacial agents dry;
When dispensing, small area or lattice are constructed, it is stirred in bucket with minitype electric mixer, often stirs and be once finished one
Whole bag;During large-area construction, stirred with special-purpose stirring machine, the method pumped with mortar is constructed;The slurry mixed should be at 30 minutes
Inside it is finished, slurry supply is timely, it is ensured that the continuity of the whole scope of operation;
Cast, working region is allowed slightly to divulge information, but door and window should be closed, and be must assure that before cast on basal plane without water, is being applied
Indoor and surface temperature should be higher than that 10 DEG C in man-hour and construction one week after;, it is necessary to wide according to the scope of operation before gravity flowing levelling mortar construction
Degree and field condition set construction joint, and cement self-leveling operation side width is no more than 6~8 meters;The Self-leveling that will be stirred
Mortar falls on basal plane, uniformly spreads out, and is struck off with special tooth mouthful scraper plate, then with mace reciprocating rolling is with profit exhaust and disappears
Except stubble is connect, treating that it is smeared from putting down, once must reach required thickness, after surface condenses, can not smear again;The strip Self-leveling of cast
Material should reach design thickness, if Self-leveling construction thickness design is less than 3mm, need to use special tooth mouthful scraper plate to be controlled
System;The auto-flowing floor that the rapid mace rolling of drift bolt footwear was poured into a mould is to discharge the air brought into during stirring, it is to avoid bubble, fiber crops
The interface discrepancy in elevation between face and bar and bar;Used instrument and equipment should be cleaned with water in time;
Maintenance, is not usually required to maintenance, if environment temperature is very high, sun direct projection, be air-dried situation if need to be conserved, will mould
Material film covered on and conserved two days in the gravity flow flat surface of firmization;
Expansion joint process, auto-flowing floor construction terminate 24 hours after, can with cutting machine stretching in substrate concrete structure
The expansion joint of 3mm is cut out at contracting seam, the expansion joint of well cutting is cleaned out, sealed with elastic sealant and filled.
2. the construction technology of a kind of imitative stone material Self-leveling waterproof mortar according to claim 1, it is characterised in that:It is described
Step(2)The crack of substrate surface will pick and dig into " V " type groove when middle basic unit has the seepage to carry out water-proofing treatment, and use Self-leveling sand
Slurry repairing is smooth, and pit, hole must also be repaired smooth with gravity flowing levelling mortar.
3. the construction technology of a kind of imitative stone material Self-leveling waterproof mortar according to claim 1, it is characterised in that:The step
Suddenly(4)Middle match ratio is that every 25 kilograms of powders add 5.5 liters of clear water, it is impossible to arbitrarily increases water, load weighted water is placed in dry
In net agitator, electric mixer is started, add whole bag self-leveling material slowly, continuous uniform ground stirring 3 ± 1 minutes, extremely
Untill forming the uniform slurry without caking, after standing 3-5 minutes, it is stirred for 1 minute, and checks the mobile performance of slurry, it is qualified to be
Can be used, mixing time can not be long, in order to avoid it is mixed into excessive air.
4. the construction technology of a kind of imitative stone material Self-leveling waterproof mortar according to claim 1, it is characterised in that:It is described to apply
During work construction technology, 5-7cm U.S. line paper wide is pasted on skirting board, after floor construction is complete, will be unnecessary with blade
U.S. line paper removal.