CN106087557A - Waterproof honeycomb Packaging Box and preparation method thereof - Google Patents

Waterproof honeycomb Packaging Box and preparation method thereof Download PDF

Info

Publication number
CN106087557A
CN106087557A CN201610436531.4A CN201610436531A CN106087557A CN 106087557 A CN106087557 A CN 106087557A CN 201610436531 A CN201610436531 A CN 201610436531A CN 106087557 A CN106087557 A CN 106087557A
Authority
CN
China
Prior art keywords
consumption
preparation
weight portion
packaging box
calcium oxide
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610436531.4A
Other languages
Chinese (zh)
Inventor
解和锋
沐磊
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tongling Feng Feng Color Printing Co Ltd
Original Assignee
Tongling Feng Feng Color Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tongling Feng Feng Color Printing Co Ltd filed Critical Tongling Feng Feng Color Printing Co Ltd
Priority to CN201610436531.4A priority Critical patent/CN106087557A/en
Publication of CN106087557A publication Critical patent/CN106087557A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of waterproof honeycomb Packaging Box and preparation method thereof, wherein, described preparation method includes: 1) styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin and bentonite are mixed, and prepares coating M1;2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box;Wherein, described styrene-acrylic emulsion relative to 100 weight portions, the consumption of described water is 10 30 weight portions, the consumption of described silica flour is 5 20 weight portions, the consumption of described polyurethane is 10 20 weight portions, the consumption of described nano calcium oxide is 15 weight portions, and described kaolinic consumption is 3 15 weight portions, and described bentonitic consumption is 3 15 weight portions.By above-mentioned design, it is achieved that can be the most waterproof, it be substantially reduced the effect of use cost and storage cost.

Description

Waterproof honeycomb Packaging Box and preparation method thereof
Technical field
The present invention relates to the production preparation field of Honey comb like package carton, in particular it relates to waterproof honeycomb Packaging Box and Preparation method.
Background technology
Honey comb like package carton is with performances such as it are the most shockproof so that its application in daily productive life is the widest General, and in actual use, because its main material is still paper, so that it has the non-water-tight limitation of paper, enter And cause in use, and often cause Honey comb like package carton to make moist and deliquescing because of factors such as humid environments, even more serious Be to may result in carton to scrap, and then considerably increase use cost and storage cost.
Therefore it provides one can be the most waterproof, it is substantially reduced the waterproof honeycomb Packaging Box of use cost and storage cost And preparation method thereof be the present invention problem of needing solution badly.
Summary of the invention
For above-mentioned prior art, it is an object of the invention to overcome in prior art Honey comb like package carton in use process In, often cause Honey comb like package carton to make moist and deliquescing because of factors such as humid environments, more seriously may result in paper Case is scrapped, and then considerably increases the problem of use cost and storage cost, thus provides the one can be the most waterproof, is substantially reduced Waterproof honeycomb Packaging Box of use cost and storage cost and preparation method thereof.
To achieve these goals, the invention provides the preparation method of a kind of waterproof honeycomb Packaging Box, wherein, described Preparation method includes:
1) styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin and bentonite are mixed, prepare coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box;Its In,
Relative to the described styrene-acrylic emulsion of 100 weight portions, the consumption of described water is 10-30 weight portion, described silica flour Consumption is 5-20 weight portion, and the consumption of described polyurethane is 10-20 weight portion, and the consumption of described nano calcium oxide is 1-5 weight Part, described kaolinic consumption is 3-15 weight portion, and described bentonitic consumption is 3-15 weight portion.
Present invention also offers a kind of waterproof honeycomb Packaging Box prepared according to preparation method described above.
By technique scheme, the present invention is by styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin It is mixed to prepare coating with bentonite according to a certain percentage, and above-mentioned prepared coating is coated on Honey comb like package carton, thus Make the Honey comb like package carton being coated with above-mentioned coating have good water resistance when actually used, substantially increase it and make By scope, and reduce use cost and storage cost.
Other features and advantages of the present invention will be described in detail in detailed description of the invention part subsequently.
Detailed description of the invention
Hereinafter the detailed description of the invention of the present invention is described in detail.It should be appreciated that described herein specifically Embodiment is merely to illustrate and explains the present invention, is not limited to the present invention.
The invention provides the preparation method of a kind of waterproof honeycomb Packaging Box, wherein, described preparation method includes:
1) styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin and bentonite are mixed, prepare coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box;Its In,
Relative to the described styrene-acrylic emulsion of 100 weight portions, the consumption of described water is 10-30 weight portion, described silica flour Consumption is 5-20 weight portion, and the consumption of described polyurethane is 10-20 weight portion, and the consumption of described nano calcium oxide is 1-5 weight Part, described kaolinic consumption is 3-15 weight portion, and described bentonitic consumption is 3-15 weight portion.
Above-mentioned design by by styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin and bentonite according to Certain proportion is mixed to prepare coating, and is coated on Honey comb like package carton by above-mentioned prepared coating, so that be coated with The Honey comb like package carton stating coating has good water resistance when actually used, substantially increases its range, and Reduce use cost and storage cost.
The present invention one preferred embodiment in, in order to make the water resistance of the waterproof honeycomb Packaging Box prepared More preferably, relative to the described styrene-acrylic emulsion of 100 weight portions, the consumption of described water is 15-25 weight portion, the consumption of described silica flour For 10-15 weight portion, the consumption of described polyurethane is 13-17 weight portion, and the consumption of described nano calcium oxide is 2-4 weight portion, Described kaolinic consumption is 5-10 weight portion, and described bentonitic consumption is 5-10 weight portion.
Described styrene-acrylic emulsion can be styrene-acrylic emulsion type commonly used in the art, such as, preferably implements in one In mode, the viscosity of described styrene-acrylic emulsion is 2000-5000cps.
The present invention another preferred embodiment in, the viscosity of described polyurethane is not less than 25000cps.
Step 1) in mixing can operate according to this area usual manner, as long as making between each raw material mixing all Even, such as, the present invention one preferred embodiment in, step 1) in mixed process can be stirring mixing, and Stir speed (S.S.) is 50-500r/min.
In a kind of embodiment being more highly preferred to, the particle diameter of described nano calcium oxide is 100-500nm.
Present invention also offers a kind of waterproof honeycomb Packaging Box prepared according to preparation method described above.
Hereinafter will be described the present invention by embodiment.In following example, described styrene-acrylic emulsion is Henkel The trade mark of brand is the commercially available product of 7199A, described polyurethane be Dongguan City three paint Chemical Co., Ltd. supply the trade mark be L- The commercially available product of 6600, described silica flour, described nano calcium oxide, described Kaolin and described bentonite are conventional commercial product.
Embodiment 1
1) by 100g styrene-acrylic emulsion, 15g water, 10g silica flour, 13g polyurethane, 2g nano calcium oxide, 5g Kaolin and 5g It is stirring mixing under conditions of 50r/min that bentonite is placed in speed, prepares coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box A1.
Embodiment 2
1) by 100g styrene-acrylic emulsion, 25g water, 15g silica flour, 17g polyurethane, 4g nano calcium oxide, 10g Kaolin and It is stirring mixing under conditions of 500r/min that 10g bentonite is placed in speed, prepares coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box A2.
Embodiment 3
1) by 100g styrene-acrylic emulsion, 20g water, 12g silica flour, 15g polyurethane, 3g nano calcium oxide, 8g Kaolin and 8g It is stirring mixing under conditions of 200r/min that bentonite is placed in speed, prepares coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box A3.
Embodiment 4
Being prepared according to the preparation method of embodiment 1, except for the difference that, the consumption of described water is 10g, described silica flour Consumption is 5g, and the consumption of described polyurethane is 10g, and the consumption of described nano calcium oxide is 1g, and described kaolinic consumption is 3g, Described bentonitic consumption is 3g, prepares waterproof honeycomb Packaging Box A4.
Embodiment 5
Being prepared according to the preparation method of embodiment 2, except for the difference that, the consumption of described water is 30g, described silica flour Consumption is 20g, and the consumption of described polyurethane is 20g, and the consumption of described nano calcium oxide is 5g, and described kaolinic consumption is 15g, described bentonitic consumption is 15g, prepares waterproof honeycomb Packaging Box A5.
Comparative example 1
Being prepared according to the preparation method of embodiment 3, except for the difference that, the consumption of described water is 5g, described silica flour Consumption is 2g, and the consumption of described polyurethane is 5g, and the consumption of described nano calcium oxide is 0.5g, and described kaolinic consumption is 1g, described bentonitic consumption is 1g, prepares Honey comb like package carton D1.
Comparative example 2
Being prepared according to the preparation method of embodiment 3, except for the difference that, the consumption of described water is 50g, described silica flour Consumption is 40g, and the consumption of described polyurethane is 40g, and the consumption of described nano calcium oxide is 10g, and described kaolinic consumption is 30g, described bentonitic consumption is 30g, prepares Honey comb like package carton D2.
Test case
After above-mentioned prepared A1-A5, D1 and D2 being respectively placed under wet environment placement 10 days, observe its water proof case, The result obtained is as shown in table 1.
Table 1
Numbering Water proof case
A1 The non-deliquescing of carton
A2 The non-deliquescing of carton
A3 The non-deliquescing of carton
A4 The slight deliquescing of carton, does not affect use
A5 The slight deliquescing of carton, does not affect use
D1 Substantially deliquescing
D2 Substantially deliquescing
The preferred embodiment of the present invention described in detail above, but, the present invention is not limited in above-mentioned embodiment Detail, in the technology concept of the present invention, technical scheme can be carried out multiple simple variant, this A little simple variant belong to protection scope of the present invention.
It is further to note that each the concrete technical characteristic described in above-mentioned detailed description of the invention, at not lance In the case of shield, can be combined by any suitable means, in order to avoid unnecessary repetition, the present invention to various can The compound mode of energy illustrates the most separately.
Additionally, combination in any can also be carried out between the various different embodiment of the present invention, as long as it is without prejudice to this The thought of invention, it should be considered as content disclosed in this invention equally.

Claims (7)

1. the preparation method of a waterproof honeycomb Packaging Box, it is characterised in that described preparation method includes:
1) styrene-acrylic emulsion, water, silica flour, polyurethane, nano calcium oxide, Kaolin and bentonite are mixed, prepare coating M1;
2) by step 1) in prepare coating M1 be coated on Honey comb like package carton, prepare waterproof honeycomb Packaging Box;Wherein,
Relative to the described styrene-acrylic emulsion of 100 weight portions, the consumption of described water is 10-30 weight portion, the consumption of described silica flour For 5-20 weight portion, the consumption of described polyurethane is 10-20 weight portion, and the consumption of described nano calcium oxide is 1-5 weight portion, institute Stating kaolinic consumption is 3-15 weight portion, and described bentonitic consumption is 3-15 weight portion.
Preparation method the most according to claim 1, wherein, relative to the described styrene-acrylic emulsion of 100 weight portions, described water Consumption is 15-25 weight portion, and the consumption of described silica flour is 10-15 weight portion, and the consumption of described polyurethane is 13-17 weight Part, the consumption of described nano calcium oxide is 2-4 weight portion, and described kaolinic consumption is 5-10 weight portion, described bentonitic Consumption is 5-10 weight portion.
Preparation method the most according to claim 1 and 2, wherein, the viscosity of described styrene-acrylic emulsion is 2000-5000cps.
Preparation method the most according to claim 1 and 2, wherein, the viscosity of described polyurethane is not less than 25000cps.
Preparation method the most according to claim 1 and 2, wherein, step 1) in mixed process be stirring mixing, and stirring speed Rate is 50-500r/min.
Preparation method the most according to claim 1 and 2, wherein, the particle diameter of described nano calcium oxide is 100-500nm.
7. the waterproof honeycomb Packaging Box prepared according to the preparation method described in any one in claim 1-6.
CN201610436531.4A 2016-06-16 2016-06-16 Waterproof honeycomb Packaging Box and preparation method thereof Pending CN106087557A (en)