CN106001400A - 一种呋喃树脂自硬砂的制备方法 - Google Patents

一种呋喃树脂自硬砂的制备方法 Download PDF

Info

Publication number
CN106001400A
CN106001400A CN201610354804.0A CN201610354804A CN106001400A CN 106001400 A CN106001400 A CN 106001400A CN 201610354804 A CN201610354804 A CN 201610354804A CN 106001400 A CN106001400 A CN 106001400A
Authority
CN
China
Prior art keywords
sand
parts
furan resin
weight
resin self
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610354804.0A
Other languages
English (en)
Inventor
孙爱琴
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hefei Tenver Precision Casting Co Ltd
Original Assignee
Hefei Tenver Precision Casting Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hefei Tenver Precision Casting Co Ltd filed Critical Hefei Tenver Precision Casting Co Ltd
Priority to CN201610354804.0A priority Critical patent/CN106001400A/zh
Publication of CN106001400A publication Critical patent/CN106001400A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种呋喃树脂自硬砂的制备方法,包括以下步骤:(1)、预处理;(2)、制备二次处理砂;(3)、将二次处理砂与混合溶液按重量比1:2.3的比例混合搅拌,除去悬浮物,过滤,得到三次处理砂;(4)、将步骤(3)中得到的三次处理砂进行水洗、烘干,得到再生砂,将再生砂与呋喃树脂、环氧树脂、磷酸、硬脂酸钠、苯磺酸按比例混合,得到新的呋喃树脂自硬砂。本发明得到的呋喃树脂自硬砂制备的砂模稳定性高,可以有效防止出现气孔、砂眼、裂纹等。

Description

一种呋喃树脂自硬砂的制备方法
技术领域
本发明属于铸造领域,具体涉及一种呋喃树脂自硬砂的制备方法。
背景技术
我国是铸造大国,在铸造时,每铸造一吨铸件约产生1.5吨铸造旧砂,我国每年的铸造旧砂产量达到5000万吨以上,很多采用掩埋的方式进行处理,现在虽然有一些呋喃树脂自硬砂旧砂回收方法,而且其中的呋喃树脂回收利用率较低,造成在再次利用时,造成硬化效果差或者容易出现缺陷。
发明内容
本发明的目的是提供一种呋喃树脂自硬砂的制备方法,可以提升旧砂中的呋喃树脂的去除率,提升再生利用的效果。
本发明通过以下技术方案实现:
一种呋喃树脂自硬砂的制备方法,包括以下步骤:
(1)、将旧砂进行破碎,过40目筛,将旧砂放入洗涤池,使用旧砂重量5倍质量分数为2%的柠檬酸溶液浸泡,浸泡过程中使用超声波进行处理,超声波频率为25-28KHz,震荡10min后,按2m3/h的流量加入质量分数为6%的氨水,氨水加入量为旧砂重量的4倍,在22℃下搅拌处理12-15min,过滤,除去滤液,得到预处理砂;
(2)、将步骤(1)处理好的预处理砂使用硅砂擦洗机处理,擦洗处理时,进料浓度为35%,将擦洗处理后的砂烘干,破碎,过40目筛,使用磁选机进行磁选处理,磁选时,磁场强度为0.75T,得到二次处理砂;
(3)、将二次处理砂与混合溶液按重量比1:2.3的比例混合搅拌,除去悬浮物,过滤,得到三次处理砂,混合溶液按重量比由以下原料制成:水100份、硫酸18份、柴油20份、烯丙基磺酸钠3.2份、十二烷基磺酸钠1.2份、松醇油4份、硝酸5份;
(4)、将步骤(3)中得到的三次处理砂进行水洗、烘干,得到再生砂;将再生砂与呋喃树脂、环氧树脂、磷酸、硬脂酸钠、苯磺酸按重量比200:1.2:0.5:0.2:0.4:0.2的比例混合,在85℃下使用覆膜砂搅拌机混合搅拌2.5h,搅拌过程中使用超声波震荡处理,超声波频率为25KHz,然后自然冷却,得到呋喃树脂自硬砂。
本发明的有益效果:本发明提供的铸造用呋喃树脂自硬砂的制备方法使用呋喃树脂自硬砂旧砂作为原料,针对呋喃树脂自硬砂旧砂呋喃树脂难以分离去除的特性,采用先使用洗涤液浸泡,然后擦洗、磁选处理,再进行浮选,并精确控制各步骤的温度及处理时间,可以明显提升呋喃树脂的去除率,经各步骤处理后再生砂的LOl<0.4%,旧砂回收利用率达到94-95%,而且再生砂制备的砂模稳定性高,可以有效防止出现气孔、砂眼、裂纹等,成品率达到98%以上,本发明的混合溶液经处理后也可以重复使用,降低了处理成本。
具体实施方式
一种呋喃树脂自硬砂的制备方法,包括以下步骤:
(1)、将旧砂进行破碎,过40目筛,将旧砂放入洗涤池,使用旧砂重量5倍质量分数为2%的柠檬酸溶液浸泡,浸泡过程中使用超声波进行处理,超声波频率为25-28KHz,震荡10min后,按2m3/h的流量加入质量分数为6%的氨水,氨水加入量为旧砂重量的4倍,在22℃下搅拌处理12-15min,过滤,除去滤液,得到预处理砂;
(2)、将步骤(1)处理好的预处理砂使用硅砂擦洗机处理,擦洗处理时,进料浓度为35%,将擦洗处理后的砂烘干,破碎,过40目筛,使用磁选机进行磁选处理,磁选时,磁场强度为0.75T,得到二次处理砂;
(3)、将二次处理砂与混合溶液按重量比1:2.3的比例混合搅拌,除去悬浮物,过滤,得到三次处理砂,混合溶液按重量比由以下原料制成:水100份、硫酸18份、柴油20份、烯丙基磺酸钠3.2份、十二烷基磺酸钠1.2份、松醇油4份、硝酸5份;
(4)、将步骤(3)中得到的三次处理砂进行水洗、烘干,得到再生砂;将再生砂与呋喃树脂、环氧树脂、磷酸、硬脂酸钠、苯磺酸按重量比200:1.2:0.5:0.2:0.4:0.2的比例混合,在85℃下使用覆膜砂搅拌机混合搅拌2.5h,搅拌过程中使用超声波震荡处理,超声波频率为25KHz,然后自然冷却,得到呋喃树脂自硬砂。

Claims (1)

1.一种呋喃树脂自硬砂的制备方法,其特征在于,包括以下步骤:
(1)、将旧砂进行破碎,过40目筛,将旧砂放入洗涤池,使用旧砂重量5倍质量分数为2%的柠檬酸溶液浸泡,浸泡过程中使用超声波进行处理,超声波频率为25-28KHz,震荡10min后,按2m3/h的流量加入质量分数为6%的氨水,氨水加入量为旧砂重量的4倍,在22℃下搅拌处理12-15min,过滤,除去滤液,得到预处理砂;
(2)、将步骤(1)处理好的预处理砂使用硅砂擦洗机处理,擦洗处理时,进料浓度为35%,将擦洗处理后的砂烘干,破碎,过40目筛,使用磁选机进行磁选处理,磁选时,磁场强度为0.75T,得到二次处理砂;
(3)、将二次处理砂与混合溶液按重量比1:2.3的比例混合搅拌,除去悬浮物,过滤,得到三次处理砂,混合溶液按重量比由以下原料制成:水100份、硫酸18份、柴油20份、烯丙基磺酸钠3.2份、十二烷基磺酸钠1.2份、松醇油4份、硝酸5份;
(4)、将步骤(3)中得到的三次处理砂进行水洗、烘干,得到再生砂;将再生砂与呋喃树脂、环氧树脂、磷酸、硬脂酸钠、苯磺酸按重量比200:1.2:0.5:0.2:0.4:0.2的比例混合,在85℃下使用覆膜砂搅拌机混合搅拌2.5h,搅拌过程中使用超声波震荡处理,超声波频率为25KHz,然后自然冷却,得到呋喃树脂自硬砂。
CN201610354804.0A 2016-05-26 2016-05-26 一种呋喃树脂自硬砂的制备方法 Pending CN106001400A (zh)