CN104957879A - Manufacturing process of stone-like light outdoor furniture desktop and material for stone-like light outdoor furniture desktop - Google Patents

Manufacturing process of stone-like light outdoor furniture desktop and material for stone-like light outdoor furniture desktop Download PDF

Info

Publication number
CN104957879A
CN104957879A CN201510285922.6A CN201510285922A CN104957879A CN 104957879 A CN104957879 A CN 104957879A CN 201510285922 A CN201510285922 A CN 201510285922A CN 104957879 A CN104957879 A CN 104957879A
Authority
CN
China
Prior art keywords
parts
weight
weight portions
resin
volume
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510285922.6A
Other languages
Chinese (zh)
Other versions
CN104957879B (en
Inventor
张俊平
陈菊燕
张可俊
刘江海
骆桂珍
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
QUANZHOU JIALILAI STONE MATERIAL ARTS & CRAFTS Co Ltd
Original Assignee
QUANZHOU JIALILAI STONE MATERIAL ARTS & CRAFTS Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by QUANZHOU JIALILAI STONE MATERIAL ARTS & CRAFTS Co Ltd filed Critical QUANZHOU JIALILAI STONE MATERIAL ARTS & CRAFTS Co Ltd
Priority to CN201510285922.6A priority Critical patent/CN104957879B/en
Publication of CN104957879A publication Critical patent/CN104957879A/en
Application granted granted Critical
Publication of CN104957879B publication Critical patent/CN104957879B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a material for a stone-like light outdoor furniture desktop. The material comprises 190-210 parts by weight of gel coat resin, 1800-1885 parts by weight of a solid material, 1100-1300 parts by weight of epoxy resin 501A, 250-270 parts by weight of epoxy resin 501B, 60-70 parts by weight of a resin foaming agent, 545-595 parts by weight of 191# resin, 180-210 parts by weight of 80FA barras, 150-200 parts by weight of an alkali-free curly grain glass fiber mat, 5-8 parts by volume of accelerant cobalt naphthenate and 2-6 parts by volume of curing agent peroxidation methyl ethyl ketone, wherein the congruent relationship of the parts by weight to the parts by volume is g/mL. According to the material, natural stone such as color sand and red river sand is sufficiently used, so that the environmental requirement is met; in addition, outdoor furniture made of the material for the stone-like light outdoor furniture desktop is firm and wear-resisting in surface, and high in weather fastness and corrosion resistance; the outdoor furniture desktop is light, convenient to transport and move and variable in model, and can imitate various materials such as wood, stone and iron; and a brand-new selection is provided for the outdoor furniture.

Description

A kind of manufacture craft of imitative stone light outdoor furniture table and material thereof
Technical field
The present invention relates to a kind of manufacture craft and material thereof of imitative stone light outdoor furniture table.
Background technology
Outdoor furniture refers in opening or semi-open property outdoor space, a series of apparatus for indoor furniture of arranging for convenience of the outdoor activities of health of people, comfortable, leisure, it mainly covers the four large series products such as the public outdoor furniture in city, garden outdoor leisure furniture, commercial location outdoor furniture, portable outdoor furniture.
Because outdoor furniture is positioned over outdoor for a long time, so have high requirements to the performance of outdoor furniture.
Be divided into wood furniture from material, metal furniture, bamboo and cane furniture, wood furniture owing to being chronically exposed to outdoor easily distortion, and needs to paint to carry out time-based maintenance; Compare with the furniture of wooden material, the furniture of metal material is more durable, but its weight is generally heavier, and not impact resistance; The outdoor furniture of bamboo rattan quality is attractive in appearance, but easily mouldyly has to pass through special treatment process, and price is higher.
Summary of the invention
The technical problem to be solved in the present invention overcomes existing defect, provides a kind of light weight, corrosion resistant Novel imitation stone light outdoor furniture table material.
In order to solve the problems of the technologies described above, the invention provides following technical scheme:
A kind of imitative stone light outdoor furniture table material, comprises each component of following number:
Epoxy resin 501A, 250 ~ 270 parts by weight epoxy resin 501B of the gel coating resin of 190 ~ 210 weight portions, the solid material of 1800 ~ 1885 weight portions, 1100 ~ 1300 weight portions, 60 ~ 70 parts by weight resin blowing agents, the 191# resin of 545 ~ 595 weight portions, the 80FA barras of 180 ~ 210 weight portions, the random line glass mat of alkali-free of 150 ~ 200 weight portions, the promoter cobalt naphthenate of 5 ~ 8 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 ~ 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
Further, this imitative stone light outdoor furniture table material, comprises each component of following number:
Resin expanded dose of the gel coating resin of 200 weight portions, the solid material of 1840 weight portions, the epoxy resin 501A 1200 parts of weight portion, epoxy resin 501B 260 parts, 65 weight portions, the 191# resin of 570 weight portions, the 80FA barras of 195 weight portions, the random line glass mats of 150 ~ 200 weight portion alkali-frees, the promoter cobalt naphthenate of 6.8 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 ~ 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
Further, described solid material comprises each component of following parts by weight:
Color 40 ~ 50 parts, the sand of 60 ~ 80 orders
Color 21.7 ~ 32 parts, the sand of 40 ~ 60 orders
10.8 ~ 16 parts, Red River sand
Stone flour 4.8 ~ 20 parts
Calomel mercurous chloride 1.3 ~ 2.5 parts
Talcum powder 3.4 ~ 8.7 parts
The plaster of paris 10.2 ~ 26.2 parts
33.3 ~ 60 parts, Snow Flower White 100 order sand.
Preferably, described solid material comprises each component of following parts by weight:
Color 45 parts, the sand of 60 ~ 80 orders
Color 25 parts, the sand of 40 ~ 60 orders
Husky 14 parts of Red River
Stone flour 12 parts
Calomel mercurous chloride 1.5 parts
Talcum powder 5 parts
The plaster of paris 18 parts
Husky 45 parts of Snow Flower White 100 order.
The manufacture craft of this imitative stone light outdoor furniture table, comprises following step:
(1) mould of cleaning for making imitative stone light outdoor furniture table, is placed on this mould on totally smooth work top;
(2) take the gel coating resin of 190 ~ 210 weight portions and the promoter cobalt naphthenate of 0.5 ~ 1 parts by volume, after stirring, then add the curing agent methyl ethyl ketone peroxide of 0.5 ~ 1 parts by volume, after mixing, pour mould blend rubber scraper plate into and strike off; Preferably, take the gel coating resin of 200 weight portions and the promoter cobalt naphthenate of 0.8 parts by volume, stir rear use
(3) solid material of 450 ~ 500 weight portions is proportionally prepared, then add the 191# resin of 230 ~ 250 weight portions, the 80FA barras of 75 ~ 85 weight portions, the promoter cobalt naphthenate of 2.0 ~ 3.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off; Preferably, take the solid material of prefabricated 480 weight portions of mixing, the 191# resin of 240 weight portions, the 80FA barras of 80 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide and mix rear use;
(4) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(5) solid material of 450 ~ 500 weight portions is proportionally prepared again, then add the 191# resin of 230 ~ 250 weight portions, the 80FA barras of 75 ~ 85 weight portions, the promoter cobalt naphthenate of 2.0 ~ 3.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off; Preferably, take the solid material of prefabricated 480 weight portions of mixing, the 191# resin of 240 weight portions, the 80FA barras of 80 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide and mix rear use;
(6) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(7) solid material of 170 ~ 185 weight portions, the 191# resin of 85 ~ 95 weight portions, the 80FA barras of 30 ~ 40 weight portions, the promoter cobalt naphthenate of 0.5 ~ 1.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide is proportionally prepared again, mix, with scraper along mould stile along smearing one deck uniformly; Preferably, proportionally take the solid material of prefabricated 180 weight portions of mixing, the 191# resin of 90 weight portions, the 80FA barras of 30 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide, mix rear use.
(8) proportionally take the prefabricated 700 parts by weight solids materials of mixing, epoxy resin 501A, 250 ~ 270 parts by weight epoxy resin 501B of 1100 ~ 1300 weight portions and 60 ~ 70 parts by weight resin blowing agents, to stir, pour mould into;
(9) back mould is buckled, static pressure 2.5 hours;
(10) form removal, static pressure are repaired product after 72 hours, repair, are painted, finally at its surface spraying last layer osmosis type anti-fouling agent.
Imitative stone light outdoor furniture table material of the present invention makes full use of the natural stone such as color sand, Red River sand and meets environmental requirement, and adopt the outdoor furniture surface hard wear resistant of this imitative stone light outdoor furniture table material, weatherability and by force corrosion-resistant, and light weight, be convenient to transport, move, moulding is changeable, can imitate wood, imitative stone, the various materials such as imitative iron, for outdoor furniture provides a kind of brand-new selection.
Detailed description of the invention
Below the preferred embodiments of the present invention are described, should be appreciated that preferred embodiment described herein is only for instruction and explanation of the present invention, is not intended to limit the present invention.
embodiment 1
A kind of imitative stone light outdoor furniture table material, comprises each component of following number:
Epoxy resin 501A, the 250 parts by weight epoxy resin 501B of the gel coating resin of 190 weight portions, the solid material of 1800 weight portions, 1100 weight portions, 60 parts by weight resin blowing agents, the 191# resin of 545 weight portions, the 80FA barras of 180 weight portions, the random line glass mat of alkali-free of 150 weight portions, the promoter cobalt naphthenate of 5 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
Described solid material comprises each component of following parts by weight:
Color 40 parts, the sand of 60 ~ 80 orders
Color 21.7 parts, the sand of 40 ~ 60 orders
Husky 10.8 parts of Red River
Stone flour 4.8 parts
Calomel mercurous chloride 1.3 parts
Talcum powder 3.4 parts
The plaster of paris 10.2 parts
Husky 33.3 parts of Snow Flower White 100 order.
A manufacture craft for imitative stone light outdoor furniture table, comprises following step:
(1) mould of cleaning for making imitative stone light outdoor furniture table, is placed on this mould on totally smooth work top;
(2) take the gel coating resin of 190 weight portions and the promoter cobalt naphthenate of 0.5 parts by volume, after stirring, then add the curing agent methyl ethyl ketone peroxide of 0.5 ~ 1 parts by volume, after mixing, pour mould blend rubber scraper plate into and strike off;
(3) solid material of 450 weight portions is proportionally prepared, then add the 191# resin of 230 weight portions, the 80FA barras of 75 weight portions, the promoter cobalt naphthenate of 2.0 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(4) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(5) solid material of 450 weight portions is proportionally prepared again, then add the 191# resin of 230 weight portions, the 80FA barras of 75 weight portions, the promoter cobalt naphthenate of 2.0 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(6) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(7) solid material of 200 weight portions, the 191# resin of 85 weight portions, the 80FA barras of 30 weight portions, the promoter cobalt naphthenate of 0.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide is proportionally prepared again, mix, with scraper along mould stile along smearing one deck uniformly;
(8) proportionally take the prefabricated 700 parts by weight solids materials of mixing, epoxy resin 501A, the 250 parts by weight epoxy resin 501B of 1100 weight portions and 60 ~ 70 parts by weight resin blowing agents, to stir, pour mould into;
(9) back mould is buckled, static pressure 2.5 hours;
(10) form removal, static pressure are repaired product after 72 hours, repair, are painted, finally at its surface spraying last layer osmosis type anti-fouling agent.
embodiment 2
A kind of imitative stone light outdoor furniture table material, comprises each component of following number:
Epoxy resin 501A, the 270 parts by weight epoxy resin 501B of the gel coating resin of 210 weight portions, the solid material of 1885 weight portions, 1300 weight portions, 70 parts by weight resin blowing agents, the 191# resin of 595 weight portions, the 80FA barras of 210 weight portions, the random line glass mat of alkali-free of 200 weight portions, the promoter cobalt naphthenate of 8 parts by volume, the curing agent methyl ethyl ketone peroxide of 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
Described solid material comprises each component of following parts by weight:
Color 50 parts, the sand of 60 ~ 80 orders
Color 32 parts, the sand of 40 ~ 60 orders
Husky 16 parts of Red River
Stone flour 20 parts
Calomel mercurous chloride 2.5 parts
Talcum powder 8.7 parts
The plaster of paris 26.2 parts
Husky 60 parts of Snow Flower White 100 order.
Its manufacture craft, comprises following step:
(1) mould of cleaning for making imitative stone light outdoor furniture table, is placed on this mould on totally smooth work top;
(2) take the gel coating resin of 210 weight portions and the promoter cobalt naphthenate of 1 parts by volume, after stirring, then add the curing agent methyl ethyl ketone peroxide of 1 parts by volume, after mixing, pour mould blend rubber scraper plate into and strike off;
(3) solid material of 500 weight portions is proportionally prepared, then add the 191# resin of 250 weight portions, the 80FA barras of 85 weight portions, the promoter cobalt naphthenate of 2.5 parts by volume and 3 weight portion methyl ethyl ketone peroxides to mix, pour mould blend rubber scraper plate into and strike off;
(4) put the random line glass mat of 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(5) solid material of 500 weight portions is proportionally prepared again, then add the 191# resin of 250 weight portions, the 80FA barras of 85 weight portions, the promoter cobalt naphthenate of 3.5 parts by volume and 1 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(6) put, the random line glass mats of 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(7) solid material of 185 weight portions, the 191# resin of 95 weight portions, the 80FA barras of 40 weight portions, the promoter cobalt naphthenate of 1 parts by volume and 1 weight portion methyl ethyl ketone peroxide is proportionally prepared again, mix, with scraper along mould stile along smearing one deck uniformly;
(8) proportionally take the prefabricated 700 parts by weight solids materials of mixing, epoxy resin 501A, the 270 parts by weight epoxy resin 501B of 1300 weight portions and 70 parts by weight resin blowing agents, to stir, pour mould into;
(9) back mould is buckled, static pressure 2.5 hours;
(10) form removal, static pressure are repaired product after 72 hours, repair, are painted, finally at its surface spraying last layer osmosis type anti-fouling agent.
embodiment 3
Resin expanded dose of the gel coating resin of 200 weight portions, the solid material of 1840 weight portions, the epoxy resin 501A 1200 parts of weight portion, epoxy resin 501B 260 parts, 65 weight portions, the 191# resin of 570 weight portions, the 80FA barras of 235 weight portions, the random line glass mats of 175 weight portion alkali-frees, the promoter cobalt naphthenate of 6.8 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 ~ 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
Described solid material comprises each component of following parts by weight:
Color 45 parts, the sand of 60 ~ 80 orders
Color 25 parts, the sand of 40 ~ 60 orders
Husky 14 parts of Red River
Stone flour 12 parts
Calomel mercurous chloride 1.5 parts
Talcum powder 5 parts
The plaster of paris 18 parts
Husky 45 parts of Snow Flower White 100 order.
The manufacture craft of imitative stone light outdoor furniture table, comprises following step:
(1) mould of cleaning for making imitative stone light outdoor furniture table, is placed on this mould on totally smooth work top;
(2) take the gel coating resin of 200 weight portions and the promoter cobalt naphthenate of 0.8 parts by volume, after stirring, then add the curing agent methyl ethyl ketone peroxide of 0.8 parts by volume, after mixing, pour mould blend rubber scraper plate into and strike off;
(3) proportionally take the solid material of prefabricated 480 weight portions of mixing, the 191# resin of 240 weight portions, the 80FA barras of 80 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(4) put the random line glass mat of 75 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(5) proportionally take the solid material of prefabricated 480 weight portions of mixing, the 191# resin of 240 weight portions, the 80FA barras of 80 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(6) put the random line glass mat of 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(7) solid material of prefabricated 180 weight portions of mixing, the 191# resin of 90 weight portions, the 80FA barras of 30 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide is proportionally taken, mix, with scraper along mould stile along smearing one deck uniformly;
(8) proportionally take the prefabricated 700 parts by weight solids materials of mixing, 1200 parts by weight epoxy resin 501A, 260 parts by weight epoxy resin 501B and 65 parts by weight resin blowing agents, to stir, pour mould into;
(9) back mould is buckled, static pressure 2.5 hours;
(10) form removal, static pressure are repaired product after 72 hours, repair, are painted, finally at its surface spraying last layer osmosis type anti-fouling agent.
Last it is noted that the foregoing is only the preferred embodiments of the present invention, be not limited to the present invention, although with reference to previous embodiment to invention has been detailed description, for a person skilled in the art, it still can be modified to the technical scheme described in foregoing embodiments, or carries out equivalent replacement to wherein portion of techniques feature.
Within the spirit and principles in the present invention all, any amendment done, equivalent replacement, improvement etc., all should be included within protection scope of the present invention.

Claims (8)

1. an imitative stone light outdoor furniture table material, is characterized in that, comprise each component of following number:
Epoxy resin 501A, 250 ~ 270 parts by weight epoxy resin 501B of the gel coating resin of 190 ~ 210 weight portions, the solid material of 1800 ~ 1885 weight portions, 1100 ~ 1300 weight portions, 60 ~ 70 parts by weight resin blowing agents, the 191# resin of 545 ~ 595 weight portions, the 80FA barras of 180 ~ 210 weight portions, the random line glass mat of alkali-free of 150 ~ 200 weight portions, the promoter cobalt naphthenate of 5 ~ 8 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 ~ 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
2. a kind of imitative stone light outdoor furniture table material as claimed in claim 1, is characterized in that, comprise each component of following number:
Resin expanded dose of the gel coating resin of 200 weight portions, the solid material of 1840 weight portions, the epoxy resin 501A 1200 parts of weight portion, epoxy resin 501B 260 parts, 65 weight portions, the 191# resin of 570 weight portions, the 80FA barras of 195 weight portions, the random line glass mats of 150 ~ 200 weight portion alkali-frees, the promoter cobalt naphthenate of 6.8 parts by volume, the curing agent methyl ethyl ketone peroxide of 2 ~ 6 parts by volume; Wherein the corresponding relation of weight portion and parts by volume is g/mL.
3. the one as described in any one of claim 1 or 2 imitates stone light outdoor furniture table material, it is characterized in that, described solid material comprises each component of following parts by weight:
Color 40 ~ 50 parts, the sand of 60 ~ 80 orders
Color 21.7 ~ 32 parts, the sand of 40 ~ 60 orders
10.8 ~ 16 parts, Red River sand
Stone flour 4.8 ~ 20 parts
Calomel mercurous chloride 1.3 ~ 2.5 parts
Talcum powder 3.4 ~ 8.7 parts
The plaster of paris 10.2 ~ 26.2 parts
33.3 ~ 60 parts, Snow Flower White 100 order sand.
4. the one as described in any one of claim 1 or 2 imitates stone light outdoor furniture table material, it is characterized in that, described solid material comprises each component of following parts by weight:
Color 45 parts, the sand of 60 ~ 80 orders
Color 25 parts, the sand of 40 ~ 60 orders
Husky 14 parts of Red River
Stone flour 12 parts
Calomel mercurous chloride 1.5 parts
Talcum powder 5 parts
The plaster of paris 18 parts
Husky 45 parts of Snow Flower White 100 order.
5. a manufacture craft for a kind of imitative stone light outdoor furniture table as described in any one of claim 1-2, is characterized in that, comprise following step:
(1) mould of cleaning for making imitative stone light outdoor furniture table, is placed on this mould on totally smooth work top;
(2) take the gel coating resin of 190 ~ 210 weight portions and the promoter cobalt naphthenate of 0.5 ~ 1 parts by volume, after stirring, then add the curing agent methyl ethyl ketone peroxide of 0.5 ~ 1 parts by volume, after mixing, pour mould blend rubber scraper plate into and strike off;
(3) solid material of 450 ~ 500 weight portions is proportionally prepared, then add the 191# resin of 230 ~ 250 weight portions, the 80FA barras of 75 ~ 85 weight portions, the promoter cobalt naphthenate of 2.0 ~ 3.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(4) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(5) solid material of 450 ~ 500 weight portions is proportionally prepared again, then add the 191# resin of 230 ~ 250 weight portions, the 80FA barras of 75 ~ 85 weight portions, the promoter cobalt naphthenate of 2.0 ~ 3.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide to mix, pour mould blend rubber scraper plate into and strike off;
(6) put the random line glass mat of 75 ~ 100 weight portion alkali-frees, pat 3 ~ 10 minutes with rubber flap;
(7) solid material of 170 ~ 185 weight portions, the 191# resin of 85 ~ 95 weight portions, the 80FA barras of 30 ~ 40 weight portions, the promoter cobalt naphthenate of 0.5 ~ 1.5 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide is proportionally prepared again, mix, with scraper along mould stile along smearing one deck uniformly;
(8) proportionally take the prefabricated 700 parts by weight solids materials of mixing, epoxy resin 501A, 250 ~ 270 parts by weight epoxy resin 501B of 1100 ~ 1300 weight portions and 60 ~ 70 parts by weight resin blowing agents, to stir, pour mould into;
(9) back mould is buckled, static pressure 2.5 hours;
(10) form removal, static pressure are repaired product after 72 hours, repair, are painted, finally at its surface spraying last layer osmosis type anti-fouling agent.
6. the manufacture craft of a kind of imitative stone light outdoor furniture table as claimed in claim 5, is characterized in that, take the gel coating resin of 200 weight portions and the promoter cobalt naphthenate of 0.8 parts by volume, stir rear use in described step (2).
7. the manufacture craft of a kind of imitative stone light outdoor furniture table as claimed in claim 5, it is characterized in that, proportionally take the solid material of prefabricated 480 weight portions of mixing, the 191# resin of 240 weight portions, the 80FA barras of 80 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide in described (3) and step (5) and mix rear use.
8. the manufacture craft of a kind of imitative stone light outdoor furniture table as claimed in claim 5, it is characterized in that, proportionally take the solid material of prefabricated 180 weight portions of mixing, the 191# resin of 90 weight portions, the 80FA barras of 30 weight portions, the promoter cobalt naphthenate of 3 parts by volume and 0.5 ~ 3 weight portion methyl ethyl ketone peroxide in described (7), mix rear use.
CN201510285922.6A 2015-05-29 2015-05-29 A kind of manufacture craft and its material of imitative stone light outdoor furniture table Active CN104957879B (en)