CN104815349B - Adhesive prepared using giant salamander mucus and preparation method thereof - Google Patents

Adhesive prepared using giant salamander mucus and preparation method thereof Download PDF

Info

Publication number
CN104815349B
CN104815349B CN201510154685.XA CN201510154685A CN104815349B CN 104815349 B CN104815349 B CN 104815349B CN 201510154685 A CN201510154685 A CN 201510154685A CN 104815349 B CN104815349 B CN 104815349B
Authority
CN
China
Prior art keywords
giant salamander
preparation
salamander mucus
adhesive
mucus
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201510154685.XA
Other languages
Chinese (zh)
Other versions
CN104815349A (en
Inventor
商海涛
王莹
陈兵
苟强
魏泓
邢孟秋
周明辉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Chongqing Changsheng Lake Fish Bio Polytron Technologies Inc
Wei Hong
Xing Mengqiu
Zhou Minghui
Original Assignee
CHONGQING KUIXU BIOLOGICAL SCIENCE & TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by CHONGQING KUIXU BIOLOGICAL SCIENCE & TECHNOLOGY Co Ltd filed Critical CHONGQING KUIXU BIOLOGICAL SCIENCE & TECHNOLOGY Co Ltd
Priority to CN201510154685.XA priority Critical patent/CN104815349B/en
Publication of CN104815349A publication Critical patent/CN104815349A/en
Application granted granted Critical
Publication of CN104815349B publication Critical patent/CN104815349B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses adhesive prepared using giant salamander mucus and preparation method thereof, adhesive is the freeze-dried powder of giant salamander mucus, its preparation method is that giant salamander mucus is frozen into solid, then vacuum freezedrying removes moisture removal, dry giant salamander mucus is crushed again, sterilizing, is produced, this method is simple, obtained adhesive bonding performance is strong, tissue adhesive can be directly used as, bonding, bone bonding for wound etc., because the adhesive derives from giant salamander, for pure natural components, security and good biocompatibility, it is degradable, it is with a wide range of applications.

Description

Adhesive prepared using giant salamander mucus and preparation method thereof
Technical field
The invention belongs to technical field of biological material, and in particular to adhesive and the adhesive prepared by a kind of utilization giant salamander mucus Preparation method.
Background technology
Giant salamander is commonly called as the giant salamander, is under the jurisdiction of Amphibia Caudata Yin Sai salamanders section, including 23 kinds of category, i.e. giant salamander category and hidden cheek salamander Category, wherein giant salamander category again can be divided into Andrias japonicus and Chinese giant salamander, Andrias davidianus, be existing maximum, the most precious amphibian in the world, by The United Nations is included in endangered species protection register, is national two classes protection aqua-marine life.Giant salamander fine and tender taste, delicious flavour, Containing good protein, abundant amino acid and trace element, nutritive value is high, is described as " ginseng in water " and " soft Huang Gold ".When giant salamander skin is by environmental stimuli, a large amount of white " milky "s, mucus with special odor can be secreted, are sent out through research Main component is water (83-86%), protein (12%) in the mucus now secreted, and containing a small amount of polysaccharide (0.48%), is had Antibacterial, it is anti-oxidant and antitumor the effects such as, cosmetic field is mainly used at present.Because the yield of giant salamander mucus is filled very much Foot, repeats a large amount of collections, and its utilization rate is low.It would therefore be highly desirable to further be developed to the addition product of giant salamander mucus, giant salamander is improved Comprehensive value.
The content of the invention
In view of this, an object of the present invention is to provide the adhesive prepared using giant salamander mucus, and bond properties is strong, Good biocompatibility, it is degradable, and security is good;The second object of the present invention is the preparation method for providing above-mentioned adhesive.
For achieving the above object, the present invention provides following technical scheme:
1st, the adhesive prepared using giant salamander mucus, described adhesive is the freeze-dried powder or vacuum drying powder of giant salamander mucus.
2nd, the preparation method of described adhesive, comprises the following steps:Giant salamander mucus is frozen into solid, then freezing vacuum Dry and remove moisture removal, then dry giant salamander mucus is crushed, sterilizing is produced.
It is preferred that, the condition of the freezing is freezed in the case where temperature is not higher than -20 DEG C.
It is preferred that, the condition of the freezing is freezed in the case where temperature is -80 DEG C~-20 DEG C.
It is preferred that, the condition of the vacuum freezedrying is less than 20Pa bars in temperature less than or equal to -50 DEG C, vacuum It is freeze-dried under part at least 48 hours.
The preparation method of the vacuum drying powder comprises the following steps:Giant salamander mucus is not higher than to 37 DEG C of condition in temperature Lower vacuum drying, then dry giant salamander mucus is crushed, sterilizing is produced.
It is preferred that, the crushing is that ultramicro grinding to particle diameter is 300~1000 mesh, and the temperature of ultramicro grinding is less than 37 DEG C i.e. Can, add liquid nitrogen and carry out ultramicro grinding best results.
It is preferred that, the sterilizing is 2~5 × 104The 60Co gamma-rays radiation sterilizations of Gy dosage.
The beneficial effects of the present invention are:The invention discloses the adhesive prepared using giant salamander mucus, the adhesive Bond properties is strong, good biocompatibility, degradable, and security is good, can act as tissue adhesive, as operation stitching etc.; The invention also discloses the preparation method of adhesive, preparation method is simple, it is not necessary to special installation, and giant salamander can be kept to glue The activity of liquid, is easy to industrialization to mass produce.
Brief description of the drawings
In order that the purpose of the present invention, technical scheme and beneficial effect are clearer, the present invention provides drawings described below:
Fig. 1 is the bonding strength measurement result of different tissues adhesive.
Fig. 2 is that tissue adhesive bonds experiment and tradition suture comparing result (A in vitro:Tissue adhesive bonds reality in vitro Test;B:Tradition suture result).
Fig. 3 is 14 days wound healing situation (A of Post operation:Tissue adhesive bonds experiment in vitro;B:Tradition suture result).
Embodiment
Below in conjunction with accompanying drawing, the preferred embodiments of the present invention are described in detail.It is unreceipted specific in embodiment The experimental method of condition, generally according to normal condition or according to the condition proposed by manufacturer.
The collection of giant salamander mucus directly scrapes sassafras method using skin:Fresh and alive giant salamander is specially cleaned into body surface with clear water, removed The impurity such as cast off a skin, be subsequently placed in dry box, giant salamander body surface is scraped with flat, until giant salamander body surface secretes a large amount of milkys Mucus, scraping was collected in culture dish, made mucus thickness about 1cm in culture dish.The collection of giant salamander mucus can also use existing Electrostimulation or etherization method collection, specific method see Publication No. 104223121A and 104206502A China specially Profit.
Embodiment 1
The method that adhesive is prepared using giant salamander mucus, is comprised the following steps:The culture dish for collecting giant salamander mucus is put -80 DEG C overnight it is frozen into solid, then with vacuum freeze drier vacuum be 19pa, temperature be -50 DEG C at freezing vacuum Dry 48 hours;Micronizer of the temperature less than 37 DEG C is placed in after lyophilized giant salamander mucus is smashed to pieces again and is crushed to 300 mesh, most Afterwards with 5 × 104Gy dosage 60Co gamma-rays radiation sterilizations, obtain tissue adhesive, aseptic packaging is standby.
Embodiment 2
The method that adhesive is prepared using giant salamander mucus, is comprised the following steps:The culture dish for collecting giant salamander mucus is put -20 DEG C overnight it is frozen into solid, then with vacuum freeze drier vacuum be 10pa, temperature be -70 DEG C at freezing vacuum Dry 56 hours;Smash lyophilized giant salamander mucus micronizer of the rearmounted temperature less than 37 DEG C to pieces again and be crushed to 500 mesh, finally With 2 × 104Gy dosage 60Co gamma-rays radiation sterilizations, obtain tissue adhesive, aseptic packaging is standby.
Embodiment 3
The method that adhesive is prepared using giant salamander mucus, is comprised the following steps:The culture dish for collecting giant salamander mucus is direct Put in vacuum drying chamber, 48h is dried under 37 DEG C of vacuum, then smash dry giant salamander mucus to pieces rearmounted temperature surpassing less than 37 DEG C Atomizer is crushed to 1000 mesh, finally with 2 × 104Gy dosage 60Co gamma-rays radiation sterilizations, obtain tissue adhesive, no bacterium bag Equipment is used.
Embodiment 4
The method that adhesive is prepared using giant salamander mucus, is comprised the following steps:The culture dish for collecting giant salamander mucus is direct Put in vacuum drying chamber, 48h is dried under 20 DEG C of vacuum, then smash dry giant salamander mucus to pieces rearmounted temperature surpassing less than 37 DEG C Atomizer is crushed to 800 mesh, finally with 2 × 104Gy dosage 60Co gamma-rays radiation sterilizations, obtain tissue adhesive, no bacterium bag Equipment is used.
Embodiment 5
External bonding experiment is carried out to adhesive made from above-described embodiment 1~4, it is specific as follows:Tried using hydraulic universal Test machine (UTM) and determine adhesive to the cohesive of pigskin, comprise the following steps that:Pig skin of back is cleaned up, take 2cm × 2 pieces of 10cm skins, remove subcutaneous fat, then in 1 piece of skin medial surface one end 2cm × 2cm area even spreads embodiment 1~4 Obtained adhesive 100mg, another piece of skin inner opposite end 2cm × 2cm area presses with finger bonding 30 seconds with the skin, so After detect bonding strength, while using Fibrin Glue and cyanoacrylate as control, as a result as shown in table 1 and Fig. 1.As a result It has been shown that, the bonding strength average out to 0.5MPa of obtained adhesive, bonding strength is far above the bonding strength of Fibrin Glue, But less than cyanoacrylate.
Table 1, the bonding strength of different adhesives are determined
Adhesive Composition Bonding strength (Mpa)
Giant salamander mucus adhesive Giant salamander mucus 0.500±0.150
Fibrin Glue Fibrinogen 5wt% 0.025±0.003
Cyanoacrylate Cyanoacrylate 0.710±0.135
It can be seen from the results above that adhesive adhesive strength produced by the present invention is high, adhesive can act as.Due to this Adhesive source is natural, and security is good, therefore can be used as tissue adhesive.
Embodiment 6
External bonding experiment is carried out to adhesive made from above-described embodiment 1~4, is specially:Using Kunming (KM) mouse as Experimental animal, takes KM mouse 18,20 ± 4g of body weight.Mouse one day before surgery is anaesthetized, shaving, depilation, second day with small Mouse mass fraction is anaesthetized for 3% yellow Jackets, with Iodophor, the ethanol disinfection operative site that volume fraction is 70%, hand Art knife is experimental group doing skin incision 2cm, left side respectively by the left and right sides of boundary of back center backbone, and right side is control Group.Experimental group is bonded using adhesive made from embodiment 1~4 to wound, and lower embodiment 1~4 is spread in wound joint Obtained adhesive 5mg, is then gently drawn with tweezers in interface both sides, as a result as shown in A in Fig. 2.As a result show, it is viscous through adhesive The visible dermis surface of a wound has been bonded together after conjunction, and surface of a wound covering sterilizing petrolatum gauze, last outside elastoplast encloses chest and abdomen Portion's wrapping one is enclosed.Control group docks skin original position, and tradition 4 pins of suture are carried out with gutstring, and the surface of a wound covers sterilizing petrolatum gauze, Last outside elastoplast encloses thorax abdomen and wraps up a circle, as shown in B in Fig. 2.Then 6 mouse sights were taken respectively in postoperative 14 days Wound healing situation is examined, as a result as shown in Figure 3.
From the figure 3, it may be seen that in situ can be healed using the mouse and tradition suture mouse wound of invention adhesives, but tradition Suture mouse healing time slower, and inflammatory reaction is substantially, scar is obvious.
Finally illustrate, preferred embodiment above is merely illustrative of the technical solution of the present invention and unrestricted, although logical Cross above preferred embodiment the present invention is described in detail, it is to be understood by those skilled in the art that can be Various changes are made to it in form and in details, without departing from claims of the present invention limited range.

Claims (8)

1. the adhesive prepared using giant salamander mucus, it is characterised in that:Described adhesive is the freeze-dried powder or vacuum of giant salamander mucus Xeraphium;
The preparation method of the freeze-dried powder comprises the following steps:Giant salamander mucus is frozen into solid, then vacuum freezedrying is gone Moisture removal, then dry giant salamander mucus is crushed, sterilizing is produced;
The preparation method of the vacuum drying powder comprises the following steps:By giant salamander mucus under conditions of temperature is not higher than 37 DEG C it is true Sky is dried, then dry giant salamander mucus is crushed, and sterilizing is produced.
2. the preparation method of claim 1 described adhesive, it is characterised in that the preparation method of the freeze-dried powder includes following step Suddenly:Giant salamander mucus is frozen into solid, then vacuum freezedrying removes moisture removal, then dry giant salamander mucus is crushed, sterilizing, Produce.
3. preparation method according to claim 2, it is characterised in that:The condition of the freezing is to be not higher than -20 in temperature Freezed at DEG C.
4. preparation method according to claim 3, it is characterised in that the condition of the freezing be temperature be -80 DEG C ~ - Freezed at 20 DEG C.
5. preparation method according to claim 2, it is characterised in that the condition of the vacuum freezedrying is small in temperature In or equal to -50 DEG C, vacuum be less than 20Pa under the conditions of be freeze-dried at least 48 hours.
6. the preparation method of adhesive according to claim 1, it is characterised in that the preparation method bag of the vacuum drying powder Include following steps:Giant salamander mucus is dried in vacuo under conditions of temperature is not higher than 37 DEG C, then dry giant salamander mucus is crushed, Sterilizing, is produced.
7. the preparation method according to any one of claim 2 ~ 6, it is characterised in that the crushing is to be less than 37 DEG C in temperature Lower ultramicro grinding to particle diameter is 300 ~ 1000 mesh.
8. the preparation method according to any one of claim 2 ~ 6, it is characterised in that the sterilizing is 2 ~ 5 × 104Gy dosage 60Co gamma-rays radiation sterilizations.
CN201510154685.XA 2015-04-02 2015-04-02 Adhesive prepared using giant salamander mucus and preparation method thereof Expired - Fee Related CN104815349B (en)