CN104624385A - 一种水锌矿与石英的浮选分离方法 - Google Patents

一种水锌矿与石英的浮选分离方法 Download PDF

Info

Publication number
CN104624385A
CN104624385A CN201510008810.6A CN201510008810A CN104624385A CN 104624385 A CN104624385 A CN 104624385A CN 201510008810 A CN201510008810 A CN 201510008810A CN 104624385 A CN104624385 A CN 104624385A
Authority
CN
China
Prior art keywords
quartz
hydrozincite
marionite
flotation separation
separation method
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510008810.6A
Other languages
English (en)
Inventor
魏宗武
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi University
Original Assignee
Guangxi University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangxi University filed Critical Guangxi University
Priority to CN201510008810.6A priority Critical patent/CN104624385A/zh
Publication of CN104624385A publication Critical patent/CN104624385A/zh
Pending legal-status Critical Current

Abstract

一种水锌矿与石英的浮选分离方法,包括如下步骤:采用硫酸调矿浆pH值为5~6,用水玻璃与直接绿作为石英矿物的抑制剂,用硫化钠及羟肟酸作水锌矿的活化剂,用十八胺醋酸钠作水锌矿的捕收剂。采用本发明能够浮选分离水锌矿与石英矿物,有效回收水锌矿,流程结构简单,药剂用量少。在给矿锌含量为8.97~12.67%条件下,经过浮选分离,获得锌含量为37.66~41.05%的氧化锌精矿,回收率为74.55%~81.60%。

Description

一种水锌矿与石英的浮选分离方法
一、技术领域
本发明涉及一种矿物浮选分离方法,特别是一种水锌矿与石英的浮选分离方法。
二、背景技术
氧化锌矿物的选矿,仍是当今国内外选矿领域中的难题之一,自上世纪以来,国内外进行了大量研究,虽然取得了一些成果,但总的来说,应用到生产中的成果较少。目前国内外氧化锌矿的回收主要采用硫胺法回收菱锌矿,即采用硫化钠先硫化,然后加胺类捕收剂进行浮选捕收,氧化锌矿的浮选回收率不高,特别是对水锌矿来说,硫胺法回收效果较差,必须加大量硫化钠对水锌矿进行硫化,然后再进行捕收;尽管如此,水锌矿的捕收效果并不理想,目前回收水锌矿的生产应用未见报道。
三、发明内容
本发明的目的在于提供一种水锌矿与石英的浮选分离方法,它能够回收水锌矿,获得较高的锌品位和回收率。
本发明采用以下技术方案达到上述目的:一种水锌矿与石英的浮选分离方法,具体步骤和药剂制度如下:
(1)用硫酸调矿浆pH值为5~6,
(2)用水玻璃与直接绿作为石英矿物的抑制剂,
(3)用硫化钠及羟肟酸作水锌矿的活化剂,
(4)用十八胺醋酸钠作水锌矿的捕收剂,
(5)浮选过程中,将矿石磨矿至矿物单体解离后,首先用硫酸调整矿浆pH值为5~6,然后加入水玻璃与直接绿抑制石英矿物,再加硫化钠及羟肟酸活化水锌矿,最后加十八胺醋酸钠对水锌矿进行捕收得到锌精矿产品,
(6)药剂总用量为:
使用时,将所述药剂先配制成以下重量百分浓度:
除另有说明外,本发明所述的百分比均为质量百分比,各组分含量百分数之和为100%。
本发明的突出优点在于:
1、能够使水锌矿与石英矿物浮选分离,在给矿锌含量为8.97~12.67%条件下,获得锌含量为37.66~41.05%的锌精矿,回收率为74.55~81.60%。
2、本发明流程结构简单,药剂用量少。
四、具体实施方式
实施例1
本发明所述的氧化锑矿物与石英的浮选分离方法的第一实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为8.97%、铁3.37%、硅35.31%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以含硅矿物为主,少量钙镁矿物及褐铁矿。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
给矿锌含量为8.97%,锌回收率达到74.55%,精矿品位37.66%。
实施例2
本发明所述的水锌矿与石英的浮选分离方法的第二实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为10.25%、铁5.60%、硅32.38%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以含硅矿物为主,少量钙镁矿物及褐铁矿。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
给矿锌含量为10.25%,锌回收率达到78.61%,精矿品位38.97%。
实施例3
本发明所述的氧化锑矿物与石英的浮选分离方法的第三实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为12.67%、铁4.83%、硅37.04%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以含硅矿物为主,少量钙镁矿物及褐铁矿。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
给矿锌含量为12.67%条件下,锌回收率达到81.60%,精矿品位41.05%。

Claims (2)

1.一种水锌矿与石英的浮选分离方法,其特征在于,具体步骤和药剂制度如下:
(1)用硫酸调矿浆pH值为5~6,
(2)用水玻璃与直接绿作为石英矿物的抑制剂,
(3)用硫化钠及羟肟酸作水锌矿的活化剂,
(4)用十八胺醋酸钠作水锌矿的捕收剂,
(5)浮选过程中,将矿石磨至单体解离后,首先用硫酸调整矿浆pH值为5~6,然后加入水玻璃与直接绿抑制石英矿物,再加硫化钠及羟肟酸活化水锌矿,最后加十八胺醋酸钠对水锌矿进行捕收得到锌精矿产品,
(6)药剂总用量为:
硫酸  1000~2000g/t
水玻璃  粗选1000~3000g/t扫选500~1000g/t  精选  300~600g/t
直接绿  粗选50~100g/t扫选20~30g/t  精选  20~30g/t
硫化钠  粗选1000~2000g/t  扫选500~1000g/t
羟肟酸  粗选200~300g/t  扫选100~200g/t
十八胺醋酸钠  粗选400~500g/t  扫选200~300g/t。
2.根据权利要求1所述的水锌矿与石英的浮选分离方法,其特征在于,使用时,将所述药剂先配制成以下重量百分浓度:
CN201510008810.6A 2015-01-08 2015-01-08 一种水锌矿与石英的浮选分离方法 Pending CN104624385A (zh)