CN104525382A - 一种水锌矿与褐铁矿的浮选分离方法 - Google Patents

一种水锌矿与褐铁矿的浮选分离方法 Download PDF

Info

Publication number
CN104525382A
CN104525382A CN201510008870.8A CN201510008870A CN104525382A CN 104525382 A CN104525382 A CN 104525382A CN 201510008870 A CN201510008870 A CN 201510008870A CN 104525382 A CN104525382 A CN 104525382A
Authority
CN
China
Prior art keywords
limonite
marionite
hydrozincite
scanned
flotation separation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510008870.8A
Other languages
English (en)
Inventor
魏宗武
穆枭
周德炎
林美群
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi University
Original Assignee
Guangxi University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangxi University filed Critical Guangxi University
Priority to CN201510008870.8A priority Critical patent/CN104525382A/zh
Publication of CN104525382A publication Critical patent/CN104525382A/zh
Pending legal-status Critical Current

Abstract

一种水锌矿与褐铁矿的浮选分离方法,包括如下步骤:用氢氧化钠调矿浆pH值为10~11,用水玻璃与木质素磺酸钠作为褐铁矿的抑制剂,用羟肟酸作水锌矿的活化剂,用氧化石腊皂及油酸钠作水锌矿的捕收剂。采用本发明能够浮选分离水锌矿与褐铁矿,流程结构简单,药剂用量少,有效回收水锌矿。在给矿锌含量为9.68~13.14%条件下,经过浮选分离,获得锌含量为36.22~38.27%的氧化锌精矿,回收率为74.07%~80.63%。

Description

一种水锌矿与褐铁矿的浮选分离方法
一、技术领域
本发明涉及一种矿物浮选分离方法,特别是一种水锌矿与褐铁矿的浮选分离方法。
二、背景技术
随着硫化锌资源逐渐减少,氧化锌矿物的选矿成为相关领域研究热点,同时也是当前国内外选矿领域中的难题之一,自上世纪以来,国内外进行了大量研究,虽然取得了一些成果,但总的来说,应用到生产中的成果较少。目前国内外对氧化锌矿回收主要限于对菱锌矿的回收,即采用硫化钠先硫化,然后加胺类捕收剂对菱锌矿进行浮选捕收,但对水锌矿的浮选回收却极少有报道,特别是水锌矿与褐铁矿的浮选分离,目前未见相关报道。
三、发明内容
本发明的目的在于提供一种水锌矿与褐铁矿的浮选分离方法,它能够回收水锌矿,获得较高的锌品位和回收率。
本发明采用以下技术方案达到上述目的:一种水锌矿与褐铁矿的浮选分离方法,具体步骤和药剂制度如下:
(1)用氢氧化钠调矿浆pH值为10~11,
(2)用水玻璃与木质素磺酸钠作为褐铁矿的抑制剂,
(3)用羟肟酸作水锌矿的活化剂,
(4)用氧化石腊皂及油酸钠作水锌矿的捕收剂,
(5)浮选过程中,将矿石磨矿至矿物单体解离后,用水力旋流器脱出-10微米细泥,再用氢氧化钠调整矿浆pH值为10~11,然后加入水玻璃与木质素磺酸钠抑制褐铁矿,再加羟肟酸活化水锌矿,最后加氧化石腊皂及油酸钠对水锌矿进行捕收得到锌精矿产品,
(6)药剂总用量为:
使用时,将所述药剂先配制成以下重量百分浓度:
除另有说明外,本发明所述的百分比均为质量百分比,各组分含量百分数之和为100%。
本发明的突出优点在于:
1、能够使水锌矿与褐铁矿浮选分离,获得锌含量为37.66~41.05%,回收率为74.55~81.60%的锌精矿。
2、本发明流程结构简单,药剂用量少。
四、具体实施方式
实施例1
本发明所述的水锌矿与褐铁矿的浮选分离方法的第一实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为9.68%、硅3.26%、铁34.63%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以褐铁矿为主,少量钙镁矿物及含硅矿物。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
锌回收率达到74.07%,精矿品位36.22%。
实施例2
本发明所述的水锌矿与褐铁矿的浮选分离方法的第二实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为11.63%、铁35.64%、硅2.30%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以褐铁矿为主,少量钙镁矿物及含硅矿物。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
锌回收率达到75.16%,精矿品位37.51%。
实施例3
本发明所述的水锌矿与褐铁矿的浮选分离方法的第三实例,包括如下步骤:
1.矿物原料:
原矿中锌品位为13.14%、铁37.50%、硅4.12%,经物相分析表明:有用矿物锌主要以水锌矿为主,少量菱锌矿、硅酸锌及异极矿;脉石矿物以褐铁矿为主,少量钙镁矿物及含硅矿物。
2、浮选流程:1次粗选、3次扫选、3次精选。
3、药剂制度及操作条件:
使用时,将所述药剂先配制成以下重量百分浓度:
4、浮选指标
锌回收率达到80.63%,精矿品位38.27%。

Claims (2)

1.一种水锌矿与褐铁矿的浮选分离方法,其特征在于,具体步骤和药剂制度如下:
(1)用氢氧化钠调矿浆pH值为10~11,
(2)用水玻璃与木质素磺酸钠作为褐铁矿的抑制剂,
(3)用羟肟酸作水锌矿的活化剂,
(4)用氧化石腊皂及油酸钠作水锌矿的捕收剂,
(5)浮选过程中,将矿石磨矿至矿物单体解离后,用水力旋流器脱出-10微米细泥,再用氢氧化钠调整矿浆pH值为10~11,然后加入水玻璃与木质素磺酸钠抑制褐铁矿,再加羟肟酸活化水锌矿,最后加氧化石腊皂及油酸钠对水锌矿进行捕收得到锌精矿产品,
(6)药剂总用量为:
氢氧化钠        1000~2000g/t
水玻璃  粗选1000~3000g/t扫选500~1000g/t精选300~600g/t
木质素磺酸钠 粗选50~100g/t扫选20~30g/t精选20~30g/t
羟肟酸   粗选200~300g/t扫选100~200g/t
油酸钠   粗选1000~2000g/t扫选500~1000g/t
氧化石腊皂  粗选400~500g/t扫选200~300g/t。
2.根据权利要求1所述的水锌矿与褐铁矿的浮选分离方法,其特征在于,使用时,将所述药剂先配制成以下重量百分浓度:
CN201510008870.8A 2015-01-08 2015-01-08 一种水锌矿与褐铁矿的浮选分离方法 Pending CN104525382A (zh)