CN103820019A - 水性聚氨酯可剥离涂料及其制备方法 - Google Patents

水性聚氨酯可剥离涂料及其制备方法 Download PDF

Info

Publication number
CN103820019A
CN103820019A CN201410082758.4A CN201410082758A CN103820019A CN 103820019 A CN103820019 A CN 103820019A CN 201410082758 A CN201410082758 A CN 201410082758A CN 103820019 A CN103820019 A CN 103820019A
Authority
CN
China
Prior art keywords
aqueous polyurethane
stripable paint
emulsifying agent
siloxanes
polyisocyanates
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410082758.4A
Other languages
English (en)
Other versions
CN103820019B (zh
Inventor
田耕
刘洪�
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
GUANGZHOU QIANSHUN INDUSTRIAL MATERIAL CO., LTD.
Original Assignee
SERVTEK MATERIAL TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SERVTEK MATERIAL TECHNOLOGY Co Ltd filed Critical SERVTEK MATERIAL TECHNOLOGY Co Ltd
Priority to CN201410082758.4A priority Critical patent/CN103820019B/zh
Publication of CN103820019A publication Critical patent/CN103820019A/zh
Application granted granted Critical
Publication of CN103820019B publication Critical patent/CN103820019B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种水性聚氨酯可剥离涂料及其制备方法,水性聚氨酯至少包括含硅氧烷的侧链。由以下物质合成:聚醚多元醇;多异氰酸酯;内乳化剂;多氨基硅氧烷;扩链剂;水。该水性聚氨酯具有很好的可剥性能和耐盐雾性能。

Description

水性聚氨酯可剥离涂料及其制备方法
技术领域
本发明涉及水性聚氨酯可剥离涂料及其制备方法。 
背景技术
许多产品在运输、装卸、组装过程中,不可避免地受到风沙、勒痕、划痕、刮痕等因素的影响,造成表面刮伤、影响美观、性能下降、甚至报废。当在材料工件表面涂一层临时保护涂料时,将避免工件损伤毁坏,完成保护后保护涂膜即可剥去,产品表面依旧能保持原有的外观和性能。可剥涂料是一种广泛用于表面临时性保护的涂料。目前,溶剂型的可剥涂料应用比较广泛,但其含有大量有机溶剂,环境友好性差;此外,热熔型的可剥涂料也有应用,但其施工难度大、能耗高;水性可剥涂料具有低VOC排放、环境友好、便于施工、保护作用强、易于剥离等优点,成为可剥涂料的一个未来发展方向。 
然而,水性聚氨酯可剥离涂料需要具有很好的分散性,要达到可剥离的效果,涂膜需要具有一定的粘结性和较好拉伸强度、断裂伸长率,这对于水性聚氨酯是个技术难题。 
发明内容
针对上述问题,本发明开发出具有很好剥离性能的水性聚氨酯可剥离涂料。 
水性聚氨酯可剥离涂料,包括水性聚氨酯,所述水性聚氨酯分子结构中的侧链至少包括含硅氧烷和内乳化剂,所述内乳化剂是具有2个羟基或氨基、且具有羧基或磺酸基的物质。 
所述的水性聚氨酯可剥离涂料由以下物质合成: 
聚醚多元醇
多异氰酸酯
内乳化剂
硅氧烷
扩链剂
所述硅氧烷为二氨基硅氧烷。
二氨基硅氧烷为N-氨乙基-3-氨丙基甲基二甲氧基硅烷,N-氨乙基-3-氨丙基乙基二甲氧基硅烷,N-氨乙基-3-氨丙基甲基二乙氧基硅烷。 
所述的多异氰酸酯选自IPDI/HDI/HMDI中的一种。 
所述的聚醚多元醇优选自聚氧化丙烯二醇、聚氧化丙烯三醇、聚四氢呋喃二醇中的一种或几种。 
以摩尔数计算,内乳化剂用量为多异氰酸酯的1%-10%。优选3%-7%。 
扩链剂为水性聚氨酯质量的0.1%-1%,大分子扩链剂用量为1%-10%。 
所述硅氧烷与内乳化剂的摩尔比为1:0.2-5。 
水性聚氨酯的制备方法,包括以下步骤: 
(1)将聚醚多元醇、部分多异氰酸酯和内乳化剂在7-10℃下搅拌混合均匀;
(2)在高速搅拌下缓慢加入多氨基硅氧烷,发生反应,形成含硅氧烷的侧链结构;
(3)反应完全后补加剩余的多异氰酸酯,升温至80℃反应得到预聚体;
(4)将预聚体缓慢加入含有扩链剂的水中,然后加入三乙胺中和,得到水性聚氨酯。
对于可剥离涂料,撕裂强度应当大于25 KN/m,断裂强度应当在10MPa以上,断裂伸长率应当在50%以上,300%以下。过低的撕裂强度、断裂强度和断裂伸长率,使得剥离涂料时不易形成一张连续的膜,而过高的断裂伸长率会导致薄膜更易吸附,导致耐盐雾降低。本申请获得的水性聚氨酯可剥离涂料具有很好的耐盐雾性能,同时具有很好的可剥性。 
  
具体实施方式
一种水性聚氨酯可剥离涂料,所述的水性聚氨酯可剥离涂料由以下物质合成: 
聚醚多元醇
多异氰酸酯
内乳化剂
二氨基硅氧烷
扩链剂
优选地,上述的二氨基硅氧烷结构如下式:
Figure 2014100827584100002DEST_PATH_IMAGE001
上式中,
R1为C-C链段和/或C-O链段;
R2、R3、R4中,其中一个为硅氧烷,其他两个独立的表示氢原子、烷基或芳烷基。
可选择的二氨基硅氧烷为N-氨乙基-3-氨丙基甲基二甲氧基硅烷,N-氨乙基-3-氨丙基乙基二甲氧基硅烷,N-氨乙基-3-氨丙基甲基二乙氧基硅烷。 
优选地,所述的多异氰酸酯选自TDI、MDI和PAPI中的一种。 
优选地,所述的聚醚多元醇优选自聚氧化丙烯二醇、聚氧化丙烯三醇、聚四氢呋喃二醇中的一种或几种。 
所述聚醚多元醇的数均分子量例如为200~8000,优选为300~5000,羟基当量例如为80~5000,优选为100~3000。 
所述的内乳化剂是指具有2个羟基或氨基、且具有羧基或磺酸基的物质,可选择的包括2,2二羟甲基丁酸,2,2二羟甲基丙酸,2,2二羟乙基丁酸,2,2二羟乙基丙酸,2,3二羟甲基丁酸,2,3二羟甲基丙酸,2,3二羟乙基丁酸,2,3二羟乙基丙酸。以摩尔数计算,内乳化剂用量为多异氰酸酯的1%-10%。优选3%-7%。 
扩链剂,本发明所述的扩链剂是指含有2个与异氰酸酯发生反应的基团,如含有2个羟基或氨基物质。扩链剂用量为水性聚氨酯预聚体质量的0.1%-1%,部分大分子扩链剂用量为1%-10%。 
本发明的水性聚氨酯的制备方法,包括以下步骤: 
(1)将聚醚多元醇、部分多异氰酸酯和内乳化剂在7-10℃下搅拌混合均匀;
(2)在高速搅拌下缓慢加入多氨基硅氧烷,发生反应,形成含硅氧烷的侧链结构;
(3)反应完全后补加剩余的多异氰酸酯,升温至80℃反应得到预聚体;
(4)将预聚体缓慢加入含有扩链剂的水中,然后加入三乙胺中和,得到水性聚氨酯。
优选地,步骤(1)的反应时间为0.5-3小时;步骤(2)的反应时间为2-6小时; 
由于氨基与异氰酸酯的反应活性比羟基与异氰酸酯的强,所以本发明采用较低温度条件下,抑制羟基与异氰酸酯的反应,以便于含有氨基的聚硅氧烷接枝到多异氰酸酯中,获得含有聚硅氧烷、含有多个异氰酸酯基团的预聚体。为了获得耐盐雾性能更好的可剥离涂料,优选二氨基硅氧烷与内乳化剂的摩尔比为1:0.2-5。
内乳化剂也可以选择含有氨基,但是内乳化剂可以在步骤(1)中的反应完全发生之后加入。可选择的含有氨基的内乳化剂包括羟甲基胺甲基丁酸、羟乙基胺乙基丁酸,二胺甲基丁酸,二胺乙基丁酸。 
氨乙基氨丙基聚二甲基硅氧烷:数均分子量3400;江西星火化工厂; 
聚氧化丙烯二醇:数均分子量2000,南京金陵石油化工厂生产;
聚氧化丙烯三醇:数均分子量1500,南京金陵石油化工厂生产;
TDI:化学纯,上海五联化工厂;
MDI:化学纯,上海五联化工厂;
三乙胺:化学纯,上海紫一试剂厂;
羟甲基氨甲基丁酸:化学纯,上海紫一试剂厂;
1,6-己二醇:化学纯,上海五联化工厂;
制备水性聚氨酯:
  实施例1 实施例2 实施例3 实施例4 实施例5 实施例6
TDI 118.5 118.5 118.5 118.5    
MDI         208.2 208.2
聚氧化丙烯二醇 159.2 159.2 159.2 159.2    
聚氧化丙烯三醇         282.7 282.7
二羟甲基丁酸 2 2        
二羟甲基丙酸        3.5 3.5 3.5
羟甲基氨甲基丁酸     3.5       
氨乙基氨丙基二甲基硅氧烷 0.2 2 1 8 0.2 2
1,6-己二醇 2 2 2 2 2 2
三乙胺 2.5 2.5 2.5 2.5 2.5 2.5
320 320 320 320 320 320
制备工艺:
(1)将聚醚多元醇、部分多异氰酸酯和内乳化剂在7-10摄氏度下搅拌混合均匀;
(2)在高速搅拌下缓慢加入多氨基硅氧烷,发生反应,形成含硅氧烷的侧链结构;
(3)反应完全后补加剩余的多异氰酸酯,升温至80℃反应得到预聚体;
(4)将预聚体缓慢加入含有扩链剂的水中,然后加入三乙胺中和,得到水性聚氨酯。
耐盐雾测试 
按照国家标准GB1771-91测试,胶膜不起泡不破损。
涂膜撕裂强度测试 
参照GB/T529-1999测试
涂膜断裂强度、断裂伸长率测试:
参照GB/T528-1998测试
 
  实施例1 实施例2 实施例3 实施例4 实施例5 实施例6
撕裂强度(KN/m) 34.8 31.5 36.2 28.3 36.7 35.1
断裂强度(M Pa) 12.5 11.3 12.4 11.5 14.5 13.2
断裂伸长率(%) 105 110 112 108 88 87
耐盐雾(h) 211 302 287 257 225 305
对于可剥离涂料,撕裂强度应当大于25 KN/m,断裂强度应当在10MPa以上,断裂伸长率应当在50%以上,300%以下。过低的撕裂强度、断裂强度和断裂伸长率,使得剥离涂料时不易形成一张连续的膜,而过高的断裂伸长率会导致薄膜更易吸附,导致耐盐雾降低。通过上述数据可以知道,本申请获得的水性聚氨酯可剥离涂料具有很好的耐盐雾性能,同时具有很好的可剥性。
  

Claims (9)

1.水性聚氨酯可剥离涂料,包括水性聚氨酯,所述水性聚氨酯分子结构中的侧链至少包括含硅氧烷和内乳化剂,所述内乳化剂是具有2个羟基或氨基、且具有羧基或磺酸基的物质。
2.根据权利要求1所述的水性聚氨酯可剥离涂料,所述的水性聚氨酯可剥离涂料由以下物质合成:
聚醚多元醇
多异氰酸酯
内乳化剂
硅氧烷
扩链剂
所述硅氧烷为二氨基硅氧烷。
3.根据权利要求2所述的水性聚氨酯可剥离涂料,二氨基硅氧烷为N-氨乙基-3-氨丙基甲基二甲氧基硅烷,N-氨乙基-3-氨丙基乙基二甲氧基硅烷,N-氨乙基-3-氨丙基甲基二乙氧基硅烷。
4.根据权利要求1所述的水性聚氨酯可剥离涂料,所述的多异氰酸酯选自TDI、MDI和PAPI中的一种。
5.根据权利要求1所述的水性聚氨酯可剥离涂料,所述的聚醚多元醇优选自聚氧化丙烯二醇、聚氧化丙烯三醇、聚四氢呋喃二醇中的一种或几种。
6.根据权利要求1所述的水性聚氨酯可剥离涂料,以摩尔数计算,内乳化剂用量为多异氰酸酯的1%-10%,优选3%-7%。
7.根据权利要求1所述的水性聚氨酯可剥离涂料,扩链剂为水性聚氨酯质量的0.1%-1%,大分子扩链剂用量为1%-10%。
8.根据权利要求1或2所述的水性聚氨酯可剥离涂料,所述硅氧烷与内乳化剂的摩尔比为1:0.2-5。
9.水性聚氨酯的制备方法,包括以下步骤:
(1)将聚醚多元醇、部分多异氰酸酯和内乳化剂在7-10℃下搅拌混合均匀;
(2)在高速搅拌下缓慢加入多氨基硅氧烷,发生反应,形成含硅氧烷的侧链结构;
(3)反应完全后补加剩余的多异氰酸酯,升温至80℃反应得到预聚体;
(4)将预聚体缓慢加入含有扩链剂的水中,然后加入三乙胺中和,得到水性聚氨酯。
CN201410082758.4A 2014-03-07 2014-03-07 水性聚氨酯可剥离涂料及其制备方法 Active CN103820019B (zh)