CN103100370B - 酒糟酸碱改性吸附材料及工艺 - Google Patents

酒糟酸碱改性吸附材料及工艺 Download PDF

Info

Publication number
CN103100370B
CN103100370B CN201110354533.6A CN201110354533A CN103100370B CN 103100370 B CN103100370 B CN 103100370B CN 201110354533 A CN201110354533 A CN 201110354533A CN 103100370 B CN103100370 B CN 103100370B
Authority
CN
China
Prior art keywords
acid
slag
vinasse
hygrometric state
modification
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201110354533.6A
Other languages
English (en)
Other versions
CN103100370A (zh
Inventor
陈彦
苏蓉蓉
林晓艳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Southwest University of Science and Technology
Original Assignee
Southwest University of Science and Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Southwest University of Science and Technology filed Critical Southwest University of Science and Technology
Priority to CN201110354533.6A priority Critical patent/CN103100370B/zh
Publication of CN103100370A publication Critical patent/CN103100370A/zh
Application granted granted Critical
Publication of CN103100370B publication Critical patent/CN103100370B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及酒糟酸碱改性吸附材料及制备工艺,采用酒糟等原料,经加酸、加碱、调配、微波加热、液渣分离、水洗、干燥等制得酒糟酸碱改性吸附材料。发明工艺不干燥酒糟,对分离洗液加以复用,改性液可用于发酵制备燃料乙醇等,制备的酒糟酸碱改性吸附材料对重金属废液中Pb2+、Cd2+、Hg2+、Cr3+、Cr6+、Ag+、Cu2+、Zn2+等的吸附脱除率约90-99%,吸附量约500mg/g。

Description

酒糟酸碱改性吸附材料及工艺
技术领域
发明涉及酒糟酸碱改性吸附材料及工艺。
背景技术
随着世界工业化的发展,重金属废液对环境和人类健康的危害日益严重。具有适用范围广、处理效果好、可回收重金属的吸附法是处理重金属废水的最有效方法之一,环境友好的生物质吸附材料具有来源广泛、成本低、可再生和易降解等特点,故近年对生物质吸附材料的研究较为活跃。中国是酒类生产和消费大国,在大规模白酒生产的同时,也产生了大量生物质废弃物——酒糟,对其的综合利用和专利主要集中于饲料、农肥、制取甘油、培养食用菌、提取复合氨基酸及微量元素等方面;以酒糟酸碱改性吸附材料用于处理重金属废液等,既可利用生物质废弃物——酒糟资源,又可改善环境。
发明内容
发明目的在于结合我国白酒生产酒糟废弃物的减量化、资源化利用与重金属废液处理实际,提供可用于重金属废液等处理的酒糟酸碱改性吸附材料及工艺。
发明的目的以如下方式实现:
以酒糟为原料,不经干燥,添加水,分别添加酸或碱进行微波加热改性,经固液分离、水洗、干燥等工艺制得。
一次调配
选用固态发酵白酒生产的丢糟——酒糟副产物,根据酒糟含水量添加水与氢氧化钠、氢氧化钾、碳酸钠、碳酸氢钠、氨水等碱改性剂中的一种,并使碱浓度约1-10%(w/w)。
微波加热
在具密闭、冷凝回流及搅拌功能的反应釜中,采用微波加热,控制在50℃-160℃下约0.5-3h。
冷却
将经微波碱处理的固液混合物自然冷却至约50-60℃。
固液分离
将冷却的固液混合物经压滤或连续离心等方式进行分离,得碱水解糖液与湿态改性渣。
水洗
添加湿态渣量1-5倍量的水并搅拌水洗、固液分离,重复水洗至中性结束。分离洗液用于一次调配,水洗中性液渣混合物用于二次调配。
二次调配
根据水洗中性液渣混合物量,添加盐酸、磷酸、硫酸、甲酸、硝酸等酸改性剂中的一种,并使酸浓度约1-10%(w/w)。
微波加热
在具密闭、冷凝回流及搅拌功能的反应釜中,采用微波加热,控制在50℃-160℃下约0.5-3h。
冷却
将经微波酸处理的固液混合物自然冷却至约50-60℃。
固液分离
将冷却的固液混合物经压滤或连续离心等方式进行分离,得酸水解糖液与湿态改性渣。
水洗
分别添加湿态渣量1-5倍量的水并搅拌水洗、固液分离,重复水洗至中性后分离结束。分离液用于二次调配,湿态渣用于干燥。
干燥
以60-100℃温度热风干燥湿态渣6-12h。
粉碎
干燥渣经低温粉碎过80目筛,即为酒糟酸碱改性吸附材料。
检验
对重金属废液中Pb2+、Cd2+、Hg2+、Cr3+、Cr6+、Ag+、Cu2+、Zn2+等的吸附脱除率约90%-99%,吸附量约500mg/g。

Claims (1)

1.一种酒糟酸碱改性吸附材料的制备方法,其特征是:采用固态发酵白酒生产的废糟——酒糟为原料,不经干燥,分别以低浓度碱、酸改性剂对酒糟进行微波加热处理,经冷却、固液分离、水洗、干燥处理进行吸附材料制备,其方法是:
1) 取样:选用固态发酵白酒生产中未经干燥预处理的丢糟——酒糟为原料;
2) 一次调配:根据酒糟含水量添加水与氢氧化钠、氢氧化钾、碳酸钠、碳酸氢钠、氨水中的一种碱改性剂,且控制碱浓度在1-10%(w/w);
3) 微波加热:在具密闭、冷凝回流及搅拌功能的反应釜中,采用微波加热,控制在50℃-160℃下0.5h -3h;
4) 冷却:将经微波碱改性处理的固液混合物自然冷却至50℃-60℃结束;
5) 固液分离:将冷却的碱改性处理的固液混合物经压滤或连续离心方式进行分离,得碱水解糖液与碱改性处理湿态渣;碱水解糖液经简单调配可直接用于发酵生产燃料乙醇;
6) 水洗:添加碱改性湿态渣量1-5倍量的水进行搅拌水洗;其分离洗液复用于一次调配;将其分离湿态渣重复水洗至中性后结束,其水洗中性液渣混合物用于二次调配;
7) 二次调配:根据水洗中性液渣混合物量,添加盐酸、磷酸、硫酸、甲酸、硝酸中的一种酸改性剂,并使酸浓度在1-10%(w/w);
8) 微波加热:在具密闭、冷凝回流及搅拌功能的反应釜中,采用微波加热,控制在50℃-160℃下0.5h-3h;
9) 冷却:将经微波酸改性处理的固液混合物自然冷却至50℃-60℃结束;
10) 固液分离:将冷却的酸改性处理固液混合物经压滤或连续离心方式进行分离,得酸水解糖液与酸改性处理湿态渣;酸水解糖液经简单调配可直接用于发酵生产燃料乙醇;
11) 水洗:添加酸改性处理湿态渣量1-5倍量的水并搅拌水洗、固液分离,重复水洗至中性后分离结束,其分离洗液复用于二次调配,其分离湿态渣用于干燥;
12) 干燥:以60℃-100℃的热风干燥湿态渣6h-12h,经此处理的渣以下称干燥渣;
13) 粉碎:将干燥渣经低温粉碎,过80目筛,即得酒糟酸碱改性吸附材料;
14) 检验:对重金属废液中Pb2+、Cd2+、Hg2+、Cr3+、Cr6+、Ag+、Cu2+、Zn2+的吸附脱率为90%-99%,吸附量500mg/g。
CN201110354533.6A 2011-11-10 2011-11-10 酒糟酸碱改性吸附材料及工艺 Expired - Fee Related CN103100370B (zh)