CN102950638B - Wood paper for painting and calligraphy and producing method thereof - Google Patents

Wood paper for painting and calligraphy and producing method thereof Download PDF

Info

Publication number
CN102950638B
CN102950638B CN201210462993.5A CN201210462993A CN102950638B CN 102950638 B CN102950638 B CN 102950638B CN 201210462993 A CN201210462993 A CN 201210462993A CN 102950638 B CN102950638 B CN 102950638B
Authority
CN
China
Prior art keywords
thin slice
wooden
wood
timber
painting
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210462993.5A
Other languages
Chinese (zh)
Other versions
CN102950638A (en
Inventor
何叶
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi fir Zhongshan Culture & Technology Development Co., Ltd.
Original Assignee
Rongshui Guangxi Snow Weasel Science And Technology Development Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Rongshui Guangxi Snow Weasel Science And Technology Development Co Ltd filed Critical Rongshui Guangxi Snow Weasel Science And Technology Development Co Ltd
Priority to CN201210462993.5A priority Critical patent/CN102950638B/en
Publication of CN102950638A publication Critical patent/CN102950638A/en
Application granted granted Critical
Publication of CN102950638B publication Critical patent/CN102950638B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a piece of wood paper for painting and calligraphy and a producing method thereof, which relate to the technical field of stationery commodities. The wood paper comprises a wood sheet layer and a reinforcing layer glued with the wood sheet layer, wherein the thickness of the wood sheet layer is smaller than 1 millimeter; and a cloth or plastic sheet is used as the reinforcing layer. The wood paper for painting and calligraphy, which has the advantages of lightness, little possibility of deforming, low cost and high quality is obtained as long as wood sheet layer is glued with the reinforcing layer by the steps of cutting selected materials, softening, slicing by planning, drying, coarsely grinding a to-be-glued face, applying glue to attach the reinforcing layer, compacting, coarsely grinding a face on which a picture is to be drawn, carrying out antiseptic, anti-discoloration and waterproof processing and finely grinding the picture face. The invention provides the producing method capable of massively producing the wood paper for painting and calligraphy.

Description

Wooden painting and calligraphy paper wood and preparation method
Technical field
The present invention relates to cultural goods technical field, paper wood and the making of the wooden painting and calligraphy that especially a kind of wood is combined with enhancement Layer.
Background technology
It is thick and heavy that this wooden painting and calligraphy paper wood has solved conventional wood panels picture materials, and consumption is large, the problem that cost is high.
It is a kind of of Chinese painting that inscribed wooden slip is drawn, ancient Chinese just has the drawing traditional habit on the wood materials such as plank, inscribed wooden slip, people are carved, are sprayed in conjunction with the natural lines of wooden grain and the processing of the art such as handwritten drawings, to people, bring spirit and visual artistic treat.And the wooden painting and calligraphy selection of prior art is batten, plank and multiple layer combination plate, be only limited to home built saw, plane, nail production intensity large, the cycle is long, how thick and heavy the wooden painting and calligraphy base material of producing is, consumption is large, cost is high, causes timber waste and yielding, carries inconvenience.
Summary of the invention
Technical problem to be solved by this invention is to provide a kind of paper wood and preparation method of light, not yielding, low-cost, high-quality wooden painting and calligraphy.
In order to address the above problem, the technical solution used in the present invention is: this wooden painting and calligraphy paper wood comprise wooden lamella and with the enhancement Layer of described wooden lamella adhesion, described wooden lamellose thickness is less than 1 millimeter; Described enhancement Layer is cloth or plastic tab;
In above-mentioned wooden painting and calligraphy paper wood technical scheme, preparation method comprises the following steps:
A, selection: choosing toothed oak wood or Chinese catalpa carpentery workshop is timber blank;
B, fracture: cut off described timber blank, making to cut off the charge length obtaining is 350 millimeters~1000 millimeters;
C, softening processing: step B cut-out is obtained to timber and be immersed in the dilution that concentration is 5%-8% timber softening agent stoste, soak 24 hours~48 hours;
D, slicing: the timber after softening is along the circumferential direction dug into the wooden thin slice of 1 millimeter~1.2 millimeters thick with slicer;
E, oven dry: put described wooden thin slice into dryer and carry out drying and processing, make the water content of ply be less than 10%;
F, corase grind rubberizing face: select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of described wooden thin slice;
G, upper gluing enhancement Layer: the floated finish at described wooden thin slice is smeared urea-formaldehyde adhesive, paste one deck enhancement Layer and make drawing paper crude product, and described enhancement Layer is cloth or plastic tab;
H, compacting: with tablet press machine, the resulting drawing paper crude product of step G is carried out to compaction treatment at normal temperatures, pressure is 2.5MPa, and be 8 seconds pressing time;
I, corase grind are made picture: the another side of the wooden thin slice of the drawing paper crude product of the wood chip sander of selecting 120 order emery wheels after to compacting carries out coarse grinding treatment, as making picture;
J, anticorrosion anti-variable color water-proofing treatment: by concentration 0 .2 % sodium hydrate aqueous solution and concentration, be successively the thin slice of the water glass solution soaking step I of 10 %~1 5 % at normal temperatures and pressures, soak time is 24 hours;
Picture is made in K, fine grinding: the wood chip sander of selection 320 order emery wheels carries out fine grinding processing to the thin slice after step J processes as picture, makes wooden lamellose thickness be less than 1 millimeter, obtains this wooden painting and calligraphy paper wood.
Owing to having adopted technique scheme, the present invention compared with prior art has following beneficial effect:
1, a kind of paper wood of light, not yielding, low-cost, high-quality wooden painting and calligraphy is provided.
2, provide a kind of and not only can carve, the paper wood of spraying, handwritten drawings, the wooden painting and calligraphy that can also print.
3, a kind of production method of wooden painting and calligraphy paper wood that can large-scale production is provided.
the specific embodiment:
Embodiment 1:
Choosing toothed oak carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 350 millimeters; Blank is immersed in the dilution that concentration is 5% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 9%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck linen and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 10 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.8 millimeter, obtains this wooden painting and calligraphy paper wood.
Embodiment 2:
Choosing and squeezing carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 1000 millimeters; Blank is immersed in the dilution that concentration is 8% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1.2 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 8%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck plastic tab and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 15 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.9 millimeter, obtains this wooden painting and calligraphy paper wood.
Embodiment 3:
Choosing and squeezing carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 800 millimeters; Blank is immersed in the dilution that concentration is 6% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1.1 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 8%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck plastic tab and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 12 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.8 millimeter, obtains this wooden painting and calligraphy paper wood.
Embodiment 4:
Choosing Chinese catalpa carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 900 millimeters; Blank is immersed in the dilution that concentration is 6% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 8%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck nylon cloth and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 12 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.8 millimeter, obtains this wooden painting and calligraphy paper wood.
Embodiment 5:
Choosing Chinese catalpa carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 350 millimeters; Blank is immersed in the dilution that concentration is 5% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1.1 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 9%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck linen and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 10 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.8 millimeter, obtains this wooden painting and calligraphy paper wood.
Embodiment 6:
Choosing Chinese catalpa carpentery workshop is timber blank; Cut off timber blank, obtain length and be the blank of 1000 millimeters; Blank is immersed in the dilution that concentration is 8% timber softening agent stoste to 24 hours; Take out the timber after softening, with slicer, timber is along the circumferential direction dug into the wooden thin slice of 1.2 millimeters thick; Put wooden thin slice into dryer and carry out drying and processing, the water content of the ply after oven dry is 8%; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of wooden thin slice; Floated finish at wooden thin slice is smeared urea-formaldehyde adhesive, pastes one deck plastic tab and forms drawing paper crude product; At normal temperatures, with tablet press machine, to pasting the drawing paper crude product obtaining, carry out compaction treatment, pressure is 2.5MPa, and be 8 seconds pressing time; Select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the exposed face of the wooden thin slice of drawing paper crude product, as making picture; Drawing paper is carried out to anticorrosion anti-variable color water-proofing treatment, successively with the water glass solution that concentration 0 .2 % sodium hydrate aqueous solution and concentration are 15 %, soak thin slice at normal temperatures and pressures, soak time is 24 hours; The wood chip sander of selecting 320 order emery wheels carries out fine grinding processing to the drawing paper after processing as picture, makes wooden lamellose thickness to 0.8 millimeter, obtains this wooden painting and calligraphy paper wood.

Claims (1)

1. a preparation method for wooden painting and calligraphy paper wood, is characterized in that comprising the following steps:
A, selection: choosing toothed oak wood or Chinese catalpa carpentery workshop is timber blank;
B, fracture: cut off described timber blank, making to cut off the charge length obtaining is 350 millimeters~1000 millimeters;
C, softening processing: step B cut-out is obtained to timber and be immersed in the dilution that concentration is 5%-8% timber softening agent stoste, soak 24 hours~48 hours;
D, slicing: the timber after softening is along the circumferential direction dug into the wooden thin slice of 1 millimeter~1.2 millimeters thick with slicer;
E, oven dry: put described wooden thin slice into dryer and carry out drying and processing, make the water content of ply be less than 10%;
F, corase grind rubberizing face: select the wood chip sander of 120 order emery wheels to carry out coarse grinding treatment to the one side of described wooden thin slice;
G, upper gluing enhancement Layer: the floated finish at described wooden thin slice is smeared urea-formaldehyde adhesive, paste one deck enhancement Layer and make drawing paper crude product, and described enhancement Layer is cloth or plastic tab;
H, compacting: with tablet press machine, the resulting drawing paper crude product of step G is carried out to compaction treatment at normal temperatures, pressure is 2.5MPa, and be 8 seconds pressing time;
I, corase grind are made picture: the another side of the wooden thin slice of the drawing paper crude product of the wood chip sander of selecting 120 order emery wheels after to compacting carries out coarse grinding treatment, as making picture;
J, anticorrosion anti-variable color water-proofing treatment: by concentration 0 .2 % sodium hydrate aqueous solution and concentration, be successively the thin slice of the water glass solution soaking step I of 10 %~1 5 % at normal temperatures and pressures, soak time is 24 hours;
Picture is made in K, fine grinding: the wood chip sander of selection 320 order emery wheels carries out fine grinding processing to the thin slice after step J processes as picture, makes wooden lamellose thickness be less than 1 millimeter, obtains this wooden painting and calligraphy paper wood.
CN201210462993.5A 2012-11-16 2012-11-16 Wood paper for painting and calligraphy and producing method thereof Active CN102950638B (en)