CN102501480B - Veneer facing mould pressing resin paint door panel and production process thereof - Google Patents
Veneer facing mould pressing resin paint door panel and production process thereof Download PDFInfo
- Publication number
- CN102501480B CN102501480B CN201110293480.1A CN201110293480A CN102501480B CN 102501480 B CN102501480 B CN 102501480B CN 201110293480 A CN201110293480 A CN 201110293480A CN 102501480 B CN102501480 B CN 102501480B
- Authority
- CN
- China
- Prior art keywords
- veneer
- door panel
- facing
- resin paint
- mould pressing
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
The invention discloses a veneer facing mould pressing resin paint door panel, which comprises a man-made board, a veneer and a synthetic resin paint film, wherein the veneer is arranged on the man-made board, and the synthetic resin paint film is coated on the veneer. The natural texture of the veneer belonging to facing materials is reserved, the stereoscopic impression of the door panel is enhanced, surface coating paint consumption is greatly reduced when the door panel is in subsequent use, labor efficiency and product quality of subsequent production are improved, production cost is reduced, the problem of environmental pollution caused by surface coating for a solid wood composite product (solid wood composite door) is thoroughly solved, and energy conservation, high efficiency and environmental protection are really realized. Industrial and large-scale production of a facing of the man-made board, particularly the man-made board (high-density mould pressing door panel) with a special-shaped surface can be realized, and the production mode of manual operation of the facing of the man-made board with the special-shaped surface is changed and realizes leap of quality and quantity. The invention further discloses a production process of the veneer facing mould pressing resin paint door panel.
Description
Technical field
The present invention relates to decorative panel technical field, particularly a kind of veneer facing mould pressing resin paint door panel and production technology thereof.
Background technology
Along with the develop rapidly of China's economic construction and improving constantly of living standards of the people, the demand of timber is increased substantially, therefore, the felling quantity of log is increasing.In order to keep ecological balance, national promotion will be greatly developed novel environment friendly material, produces with the substitute wood product that give up, and saves limited timber resources.In the last few years, various wood-based plate, the fiberboards that utilize crops and string thereof to produce occurred in succession, and preparation method is also varied.
At present, ripe veneer face artificial board production Technology be by the veneer veneer of unlike material and base material-various wood-based plates after certain technical finesse (as: balancing water content, surface coating, veneer cutting etc.), veneer veneer table is overlayed on to wood-based plate surface by the requirement having designed again, finally by a kind of production technology of high temperature, high pressure or the dalle that is only under high pressure composited.
The application mode of traditional veneer face artificial board maturation is: veneer face artificial board is cut, is combined into processing work on request, and carry out after the polishing, sanding of entirety or parts, spraying 2-3 is all over priming paint, 2-3 is all over finish paint, paint of every spray all will be polished, sanding is to meeting spraying requirement, until reach product and reach the effect of veneer facing.
Veneer face artificial board is a kind of building materials that are widely used in the field such as furniture, interior decoration decoration, use this product to carry out after furniture processing and indoor decorating, also must carry out lacquer painting covering with paint and just can reach the ideal effect that veneer veneer is decorated, but the complex process that lacquer painting is covered with paint, lacquer, colour wash, etc., paint consumption is large, and cost is high, and efficiency is low, the cycle is long, hardness of paint film is poor, and especially environmental pollution is serious.And most wood processing enterprises, lacquer painting covering with paint, polishing, sanding are the bottlenecks of its production capacity.
Therefore, how to reduce paint and consume, reduce costs, raise labour efficiency, shorten the production cycle, reduce environmental pollution, reach the effect of lacquer painting facing simultaneously, become those skilled in the art's important technological problems urgently to be resolved hurrily.
Summary of the invention
In view of this, the invention provides a kind of veneer facing mould pressing resin paint door panel and production technology thereof, consume, reduce costs, raise labour efficiency, shorten the production cycle, reduce environmental pollution to reduce paint, reach the effect of lacquer painting facing simultaneously.
For achieving the above object, the invention provides following technical scheme:
A kind of veneer facing mould pressing resin paint door panel, comprising:
Wood-based plate;
Be arranged at the veneer veneer on described wood-based plate;
Be coated on the synthetic resin paint film on described veneer veneer.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel, also comprise the nonwoven being arranged between described wood-based plate and described veneer veneer.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel, described nonwoven is bonded on described wood-based plate by synthetic resin glue-line.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel, the thickness of described veneer veneer is 0.15-0.5mm.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel, described veneer veneer is the veneer veneer of moisture content at 6-10%.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel, described wood-based plate is to have abnormally-structured wood-based plate.
A kind of veneer facing mould pressing resin paint door panel production technology, comprises step:
1) be 0.15-0.5mm by thickness, moisture content carries out selection at the veneer veneer containing nonwoven of 6-10%, and is cut into the sheet of veneer of door face board shape;
2) described sheet of veneer is pressed to 30-45g/m
2glue-spread gluing;
3) the sheet of veneer table after gluing is overlayed on to the surface that balancing water content is the wood-based plate of 6-10%;
4) it is in 130-150 DEG C, the pressure press that is 10-15MPa that the wood-based plate that table is covered with to sheet of veneer is sent into temperature, is combined into veneer facing molding fiberboard through the mold pressing of 30-60S;
5) look processing is polished, repaired and repaiies on veneer facing molding fiberboard surface, equilibrium moisture content is to 6-10%, at its front surface spray 100-200g/m
2synthetic resin, when after curable synthetic resin, form layer of smooth, hard, uniform synthetic resin paint film on its surface;
6) it is dry in the environment of 100-150 DEG C that the veneer facing molding fiberboard that surface is scribbled to synthetic resin is sent into temperature;
7) dried veneer facing molding fiberboard being sent into temperature is that in 140-180 DEG C, the pressure press die that is 15-22MPa, hot pressing 60-90s, forms veneer facing mould pressing resin paint door panel.
Preferably, in above-mentioned veneer facing mould pressing resin paint door panel production technology, described step 6) being specially the veneer facing molding fiberboard that surface is scribbled to synthetic resin, to send into temperature be dry 30S in the environment of 100-150 DEG C.
Can find out from above-mentioned technical scheme, veneer facing mould pressing resin paint door panel provided by the invention, not only retain the native texture that finishing material-veneer veneer itself has, third dimension strengthens, also greatly reduce goods in the time of follow-up use, paint amount for top finishing (or without paint), not only improved subsequent production efficiency, product quality, reduced production cost, thoroughly solution solid wood composite article (solid-wood composite wooden door) carries out the problem of environmental pollution of top finishing, has really realized energy-conservation, efficient, environmental protection.The present invention can realize wood-based plate and particularly have industrialization, the large-scale production of Special-Shaped Surface wood-based plate (high-density molded door skin) facing; solve the production model of traditional handwork with Special-Shaped Surface artificial board decorative, made it to realize leaping of quality and quantity.
Brief description of the drawings
In order to be illustrated more clearly in the embodiment of the present invention or technical scheme of the prior art, to the accompanying drawing of required use in embodiment or description of the Prior Art be briefly described below, apparently, accompanying drawing in the following describes is only some embodiments of the present invention, for those of ordinary skill in the art, do not paying under the prerequisite of creative work, can also obtain according to these accompanying drawings other accompanying drawing.
The structural representation of the veneer facing mould pressing resin paint door panel that Fig. 1 provides for the embodiment of the present invention;
The flow chart of the veneer facing mould pressing resin paint door panel production technology that Fig. 2 provides for the embodiment of the present invention.
Detailed description of the invention
The invention discloses a kind of veneer facing mould pressing resin paint door panel and production technology thereof, consume, reduce costs, raise labour efficiency, shorten the production cycle, reduce environmental pollution to reduce paint, reach the effect of lacquer painting facing simultaneously.
Below in conjunction with the accompanying drawing in the embodiment of the present invention, the technical scheme in the embodiment of the present invention is clearly and completely described, obviously, described embodiment is only the present invention's part embodiment, instead of whole embodiment.Based on the embodiment in the present invention, those of ordinary skill in the art, not making the every other embodiment obtaining under creative work prerequisite, belong to the scope of protection of the invention.
Refer to Fig. 1, the structural representation of the veneer facing mould pressing resin paint door panel that Fig. 1 provides for the embodiment of the present invention.
Veneer facing mould pressing resin paint door panel provided by the invention comprises wood-based plate 5, veneer veneer 2 and synthetic resin paint film 1.Wherein, veneer veneer 2 is arranged on wood-based plate 5, and synthetic resin paint film 1 is coated on veneer veneer 2.The invention provides veneer facing mould pressing resin paint door panel solved veneer face artificial board after continuous with time the simple lacquer painting that relies on cover with paint, lacquer, colour wash, etc. to reach its finishing effect, the problem that paint consumption is large, cost is high, efficiency is low, the cycle is long.
The present invention is based on reducing paint consumption, reduce costs, raise labour efficiency, shorten the thought of production cycle, first by veneer veneer 2 and the once molding formed fiberboard of base material through certain technical finesse (as: balancing water content, surface coating, veneer cutting etc.), and by the requirement having designed, veneer veneer 2 tables are overlayed on to wood-based plate 5 surfaces, through high temperature, high pressure " secondary " mold pressing is composited after veneer facing molding fiberboard, again synthetic resin is sprayed on the surface of veneer facing molding fiberboard, when the synthetic resin on veneer facing molding fiberboard surface is dried to while meeting the requirements, sent into again press, at high temperature, under the condition of high pressure, " three times " mold pressing veneer facing mould pressing resin paint door panel that is composited.
Veneer facing mould pressing resin paint door panel provided by the invention, not only retain the native texture that finishing material-veneer veneer 2 has itself, third dimension strengthens, also greatly reduce goods in the time of follow-up use, paint amount for top finishing (or without paint), not only improved subsequent production efficiency, product quality, reduced production cost, thoroughly solution solid wood composite article (solid-wood composite wooden door) carries out the problem of environmental pollution of top finishing, has really realized energy-conservation, efficient, environmental protection.The present invention can realize wood-based plate and particularly have industrialization, the large-scale production of Special-Shaped Surface wood-based plate (high-density molded door skin) facing; solve the production model of traditional handwork with Special-Shaped Surface artificial board decorative, made it to realize leaping of quality and quantity.
The present invention also can comprise the nonwoven 3 being arranged between wood-based plate 5 and veneer veneer 2, on veneer veneer 2, pastes layer of non-woven fabric 3, and nonwoven 3 can be bonded on wood-based plate 5 by synthetic resin glue-line 4.The thickness of veneer veneer 2 is 0.15-0.5mm, and veneer veneer 2 is the veneer veneer of moisture content at 6-10%, and in embodiments of the present invention, wood-based plate 5 can be has abnormally-structured wood-based plate.
Refer to Fig. 2, the flow chart of the veneer facing mould pressing resin paint door panel production technology that Fig. 2 provides for the embodiment of the present invention.
The production technology of veneer facing mould pressing resin paint door panel provided by the invention, comprising:
Step S1: selection is also cut into sheet of veneer;
Be first 0.15-0.5mm by thickness, moisture content carries out selection at the veneer veneer (containing nonwoven) of 6-10%, and is cut into the sheet of veneer of certain specification and figure (door face board shape).
Step S2: gluing;
Sheet of veneer is pressed to 30-45g/m
2glue-spread gluing after display, stand-by.
Step S3: table covers wood-based plate;
Sheet of veneer table after treatment gluing is overlayed on to the molded fiber plate that balancing water content is 6-10% (being wood-based plate) surface.
Step S4: mold pressing is combined into veneer facing molding fiberboard;
It is in 130-150 DEG C, the pressure press that is 10-15MPa that the molded fiber plate that table is covered with to sheet of veneer is sent into temperature, is combined into veneer facing molding fiberboard through the mold pressing of 30-60S.
Step S5: veneer facing molding fiberboard spray synthetic resin;
(polishing, repair, repair look etc.) processed in veneer facing molding fiberboard surface, and equilibrium moisture content is to 6-10%, at its front surface (having the surface of veneer veneer one side) spray 100-200g/m
2synthetic resin, when after curable synthetic resin, form layer of smooth, hard, uniform synthetic resin paint film on its surface, replace the priming paint in the follow-up use process of veneer facing fiberboard with this.
Step S6: dry processing;
It is in the environment of 100-150 DEG C that the veneer facing molding fiberboard that surface is scribbled to synthetic resin is sent into temperature, dry 30S.
Step S7: be hot pressed into veneer facing mould pressing resin paint door panel;
It is that in 140-180 DEG C, the pressure press die that is 15-22MPa, hot pressing 60-90s, can form veneer facing mould pressing resin paint door panel that dried veneer facing molding fiberboard is sent into temperature.
In sum, tool of the present invention has the following advantages:
1) the present invention can realize wood-based plate and particularly have industrialization, the large-scale production of Special-Shaped Surface wood-based plate (high-density molded door skin) facing, solve the production model of traditional handwork with Special-Shaped Surface artificial board decorative, made it to realize leaping of quality and quantity;
2) the present invention is on the basis of patent of invention " solid wood composite coining door panel and production technology ", utilizes the principle of Surface decorated woodbased panels with paper impregnated thermosetting resins, to its follow-up reprocessing, processing;
3) product of the present invention has not only retained the native texture that finishing material-veneer veneer itself has, third dimension strengthens, also greatly reduce goods in the time of follow-up use, paint amount for top finishing (or without paint), not only improved subsequent production efficiency, product quality, reduced production cost, thoroughly solution solid wood composite article (solid-wood composite wooden door) carries out the problem of environmental pollution of top finishing, has really realized energy-conservation, efficient, environmental protection.
In this description, each embodiment adopts the mode of going forward one by one to describe, and what each embodiment stressed is and the difference of other embodiment, between each embodiment identical similar part mutually referring to.
To the above-mentioned explanation of the disclosed embodiments, make professional and technical personnel in the field can realize or use the present invention.To be apparent for those skilled in the art to the multiple amendment of these embodiment, General Principle as defined herein can, in the situation that not departing from the spirit or scope of the present invention, realize in other embodiments.Therefore, the present invention will can not be restricted to these embodiment shown in this article, but will meet the widest scope consistent with principle disclosed herein and features of novelty.
Claims (2)
1. a veneer facing mould pressing resin paint door panel production technology, is characterized in that, comprises step:
1) be 0.15-0.5mm by thickness, moisture content carries out selection at the veneer veneer containing nonwoven of 6-10%, and is cut into the sheet of veneer of door face board shape;
2) described sheet of veneer is pressed to 30-45g/m
2glue-spread gluing;
3) the sheet of veneer table after gluing is overlayed on to the surface that balancing water content is the wood-based plate of 6-10%;
4) it is in 130-150 DEG C, the pressure press that is 10-15MPa that the wood-based plate that table is covered with to sheet of veneer is sent into temperature, is combined into veneer facing molding fiberboard through the mold pressing of 30-60S;
5) look processing is polished, repaired and repaiies on veneer facing molding fiberboard surface, equilibrium moisture content is to 6-10%, at its front surface spray 100-200g/m
2synthetic resin, when after curable synthetic resin, form layer of smooth, hard, uniform synthetic resin paint film on its surface;
6) it is dry in the environment of 100-150 DEG C that the veneer facing molding fiberboard that surface is scribbled to synthetic resin is sent into temperature;
7) dried veneer facing molding fiberboard being sent into temperature is that in 140-180 DEG C, the pressure press die that is 15-22MPa, hot pressing 60-90s, forms veneer facing mould pressing resin paint door panel.
2. veneer facing mould pressing resin paint door panel production technology as claimed in claim 1, is characterized in that, described step 6) is specially the veneer facing molding fiberboard that surface is scribbled to synthetic resin, and to send into temperature be dry 30S in the environment of 100-150 DEG C.