CN102886346A - Ultraviolet light (UV) cured coating pine oil seal roller-coat coating construction technology - Google Patents

Ultraviolet light (UV) cured coating pine oil seal roller-coat coating construction technology Download PDF

Info

Publication number
CN102886346A
CN102886346A CN2011102022302A CN201110202230A CN102886346A CN 102886346 A CN102886346 A CN 102886346A CN 2011102022302 A CN2011102022302 A CN 2011102022302A CN 201110202230 A CN201110202230 A CN 201110202230A CN 102886346 A CN102886346 A CN 102886346A
Authority
CN
China
Prior art keywords
roller
ultraviolet light
paint
priming paint
coating
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2011102022302A
Other languages
Chinese (zh)
Other versions
CN102886346B (en
Inventor
周靖洋
刘志刚
周琼辉
蔡晓琴
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanghai Fuchen Chemical Co Ltd
Original Assignee
Shanghai Fuchen Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanghai Fuchen Chemical Co Ltd filed Critical Shanghai Fuchen Chemical Co Ltd
Priority to CN201110202230.2A priority Critical patent/CN102886346B/en
Publication of CN102886346A publication Critical patent/CN102886346A/en
Application granted granted Critical
Publication of CN102886346B publication Critical patent/CN102886346B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides an ultraviolet light (UV) cured coating pine oil seal roller-coat coating construction technology, wherein the technology is characterized by consisting of the following steps: (1), performing material treatment; (2), roller-coating or spraying water-based oil seal priming paint (3), performing infrared leveling, (4), rolling IV priming paint, (5), performing semi-curing, (6), rolling UV priming paint, (7), performing full curing, (8), polishing, (9), performing dust removing, (10), making UV surface, (11), performing full curing, and (12), detecting and packaging. The technology provided by the invention has the following advantages that the production efficiency is high; the crack is avoided under either low-temperature condition or high-temperature condition after coating, the adhesive power is excellent, the surface rigidity is high, the color is natural, the figures are clear, and the oil-splitting phenomenon is avoided.

Description

The coating material solidified pine oil sealing of ultraviolet light (UV) roller coat coating construction process
Technical field
The present invention relates to a kind of ultraviolet light (UV) coating material solidified, refer in particular to the coating material solidified pine oil sealing of ultraviolet light (UV) roller coat coating construction process.
Background technology
On the cultural history of furniture, the Nordic intention of the founder of pine furniture is performed meritorious deeds never to be obliterated, they turn the foul and rotten into the rare and ethereal, log is become high-quality sheet material by the quick growing species of trees that excess resin crowds through the tread flaking oven dry, thereby allow pine with its simple and unadorned texture, lifelike texture, pure beautiful color and luster, domestic environment decorate plainly, pure quiet, incorporate with the harmony of nature with peaceful, thereby pine furniture united state humanity section is decided to be environmental protection furniture.Pine furniture visually elder generation's " look " is taken the people by force.Indifferent to fame or gain soft pine true qualities " the natural beauty difficulty is given up as hopeless " allow the low eyebrow of other seeds bow one's head.Not adding overwrought pine true qualities furniture is natural views, is the nature landscape, the texture that essence is spacious, fine and smooth lines, hard and soft double Ji.But unique shortcoming of pine furniture is: tell oil serious, do not choose suitable technique and coating and can make material tell oil, cause adhering between material and skin of paint bad, affect the paint quality of furniture.Therefore demand designing the paint ply adhesion that new technique is improved pine furniture urgently.
Summary of the invention
The objective of the invention is to overcome the problem of telling poor adhesive force between the oily skin of paint that seriously causes in the existing technique because of pine furniture, the coating material solidified pine oil sealing of a kind of ultraviolet light (UV) roller coat coating construction process is provided.The present invention designs the coating material solidified pine oil sealing of ultraviolet light (UV) roller coat coating construction process, it is characterized in that being comprised of the following step:
(1) material is processed: with 240# sand paper jettisoning surface burr,
(2) roller or spraying water-based oil sealing priming paint: will paint Shanghai cotton machine roller coat or with the rifle spray, suitable quantity of water latting drown when rifle sprays, single roller one time, coating weight 20-25g m 2, select similar commercially available water-based oil sealing priming paint on the model VW267A of the rich minister Chemical Manufacture in Shanghai or the market,
(3) infrared levelling: cross 3~4min with 40 ℃~45 ℃ infrared leveling machines,
(4) roller UV priming paint: single roller one time, coating weight 30-35g m 2, select similar commercially available UV priming paint on the model VU2020L of the rich minister Chemical Manufacture in Shanghai or the market, will paint winter with tank and heat 40 ℃~60 ℃,
(5) semi-solid preparation: ultraviolet light 140 ± 20mj/cm2 shines 3-4 second,
(6) roller UV priming paint: single roller one time, coating weight 30-35g m 2, select similar commercially available UV priming paint on the model VU2020L of the rich minister Chemical Manufacture in Shanghai or the market, will paint winter with tank and heat 40 ℃~60 ℃,
(7) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(8) polishing: 320# sand paper hand mill or machine polishing to surface get final product without bright spot,
(9) dedusting: with machine or artificial dedusting,
(10) do the UV face: ultraviolet light roller coat dull finishing coat, coating weight 20-25g m 2, select similar commercially available UV finish paint on the model UV3020-6N of the rich minister Chemical Manufacture in Shanghai or the market,
(11) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(12) detect packing.
Advantage of the present invention is that production efficiency is high, does not all ftracture under low temperature or high temperature after the application, and adhesive force is good, and case hardness is high, and color and luster is natural, and clean mark and nothing are told oily phenomenon.
Below in conjunction with example the present invention is elaborated.
The specific embodiment
Embodiment 1:
(1) material is processed: with 240# sand paper jettisoning surface burr,
(2) roller or spraying water-based oil sealing priming paint: the model VW267A with the rich minister Chemical Manufacture in Shanghai will paint Shanghai cotton machine roller coat, single roller one time, and coating weight 20-25g m2,
(3) infrared levelling: cross 3~4min with 40 ℃~45 ℃ infrared leveling machines and get final product,
(4) roller UV priming paint: the model VU2020L with the rich minister Chemical Manufacture in Shanghai, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(5) semi-solid preparation: ultraviolet light 140 ± 20mj/cm2 shines 3-4 second,
(6) roller UV priming paint: the model VU2020L with the rich minister Chemical Manufacture in Shanghai, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(7) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(8) polishing: 320# sand paper hand mill or machine polishing, until the surface gets final product without bright spot,
(9) dedusting: with machine or artificial,
(10) do the UV face: with the model UV3020-6N ultraviolet light roller coat dull finishing coat of the rich minister Chemical Manufacture in Shanghai, coating weight 20-25g m2,
(11) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(12) detect packing.
Embodiment 2:
(1) material is processed: with 240# sand paper jettisoning surface burr
(2) roller or spraying water-based oil sealing priming paint: the model VW267A water-based oil sealing priming paint with the rich minister Chemical Manufacture in Shanghai adds the suitable quantity of water latting drown, with rifle spray one time, and coating weight 20-25g m2,
(3) infrared levelling: cross 3~4min with 40 ℃~45 ℃ infrared leveling machines and get final product,
(4) roller UV priming paint: the model VU2020L with the rich minister Chemical Manufacture in Shanghai, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(5) semi-solid preparation: ultraviolet light 140 ± 20mj/cm2 shines 3-4 second,
(6) roller UV priming paint: the model VU2020L with the rich minister Chemical Manufacture in Shanghai, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(7) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(8) polishing: 320# sand paper hand mill or machine are polished to the surface and get final product without bright spot,
(9) dedusting: with machine or artificial dedusting,
(10) do the UV face: with the model UV3020-5D ultraviolet light roller coat dull finishing coat of the rich minister Chemical Manufacture in Shanghai, coating weight 20-25g m2,
(11) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(12) detect packing.
Embodiment 3:
(1) material is processed: with 240# sand paper jettisoning surface burr,
(2) roller or spraying water-based oil sealing priming paint: the water-based oil sealing priming paint with commercially available on the market, will paint Shanghai cotton machine roller coat, single roller one time, coating weight 20-25g m2,
(3) infrared levelling: cross 3~4min with 40 ℃~45 ℃ infrared leveling machines and get final product,
(4) roller UV priming paint: with UV priming paint commercially available on the market, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(5) semi-solid preparation: ultraviolet light 140 ± 20mj/cm2 shines 3-4 second,
(6) roller UV priming paint: with UV priming paint commercially available on the market, will paint winter with tank and heat 40 ℃~60 ℃, single roller one time, coating weight 30-35g m2,
(7) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(8) polishing: 320# sand paper hand mill or machine are polished to the surface and get final product without bright spot,
(9) dedusting: with machine or artificial dedusting,
(10) do the UV face: with UV finish paint commercially available on the market, roller coat dull finishing coat, coating weight 20-25g m2,
(11) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(12) detect packing.

Claims (1)

1. the coating material solidified pine oil sealing of ultraviolet light (UV) roller coat coating construction process is characterized in that being comprised of the following step:
(1) material is processed: with 240# sand paper jettisoning surface burr,
(2) roller or spraying water-based oil sealing priming paint: will paint Shanghai cotton machine roller coat or with the rifle spray, suitable quantity of water latting drown when rifle sprays, single roller one time, coating weight 20-25g m 2, select similar commercially available water-based oil sealing priming paint on the model VW267A of the rich minister Chemical Manufacture in Shanghai or the market,
(3) infrared levelling: cross 3~4min with 40 ℃~45 ℃ infrared leveling machines,
(4) roller UV priming paint: single roller one time, coating weight 30-35g m 2, select similar commercially available UV priming paint on the model VU2020L of the rich minister Chemical Manufacture in Shanghai or the market, will paint winter with tank and heat 40 ℃~60 ℃,
(5) semi-solid preparation: ultraviolet light 140 ± 20mj/cm2 shines 3-4 second,
(6) roller UV priming paint: single roller one time, coating weight 30-35g m 2, select similar commercially available UV priming paint on the model VU2020L of the rich minister Chemical Manufacture in Shanghai or the market, will paint winter with tank and heat 40 ℃~60 ℃,
(7) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(8) polishing: 320# sand paper hand mill or machine polishing to surface get final product without bright spot,
(9) dedusting: with machine or artificial dedusting,
(10) do the UV face: ultraviolet light roller coat dull finishing coat, coating weight 20-25g m 2, select similar commercially available UV finish paint on the model UV3020-6N of the rich minister Chemical Manufacture in Shanghai or the market,
(11) full curing: ultraviolet light 350 ± 50mj/cm2 shines 3-4 second,
(12) detect packing.
CN201110202230.2A 2011-07-19 2011-07-19 Ultraviolet light (UV) cured coating pine oil seal roller-coat coating construction technology Active CN102886346B (en)