CN102320807A - 轻质防火保温板的加工方法 - Google Patents

轻质防火保温板的加工方法 Download PDF

Info

Publication number
CN102320807A
CN102320807A CN2011102082407A CN201110208240A CN102320807A CN 102320807 A CN102320807 A CN 102320807A CN 2011102082407 A CN2011102082407 A CN 2011102082407A CN 201110208240 A CN201110208240 A CN 201110208240A CN 102320807 A CN102320807 A CN 102320807A
Authority
CN
China
Prior art keywords
sodium methyl
parts
water glass
lightweight fireproof
methyl silicate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2011102082407A
Other languages
English (en)
Other versions
CN102320807B (zh
Inventor
李金峰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JIANGSU JIANGZHONG GROUP CO Ltd
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 201110208240 priority Critical patent/CN102320807B/zh
Publication of CN102320807A publication Critical patent/CN102320807A/zh
Application granted granted Critical
Publication of CN102320807B publication Critical patent/CN102320807B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种轻质防火保温板及其加工方法,通过将以下重量份的各组份组成:膨胀珍珠岩10-30份,甲基硅酸钠1-3份,水玻璃2-6份,进行一系列的加工制备而成。本发明的优点是:通过对膨胀珍珠岩的粒径进行筛选,然后为原材料进行加工,大大降低了保温板的重量,提高了保温效果,防潮效果明显,通过甲基硅酸钠和水玻璃的充分混合后,大大提高了珍珠岩颗粒之间的粘合力;同时由于加固框的作用,提高了保温板韧度,不易发生脆裂,使得抗拉强度大大提高。

Description

轻质防火保温板的加工方法
技术领域
本发明涉及轻质防火保温板的加工方法,属于建筑材料领域。
背景技术
目前使用保温板,不具备防火的功能,有的虽然可以防火,但是防火性能较差,不能满足实际的需求,他们通常采用水泥和聚苯乙烯颗粒混合进行加工而成,具有较大的重量,容易发生脆断,造成坠落;而且聚苯乙烯颗粒对环境具有一定的影响,不环保。
发明内容
为克服现有技术的缺陷,本发明提供一种粘度系数大、不易发生脆裂、对环境无污染和耐高温的轻质防火保温板及其加工方法。本发明的技术方案是:一种轻质防火保温板,其特征在于,包括以下重量份的各组份组成:膨胀珍珠岩  10-30份,甲基硅酸钠 1-3份, 水玻璃 2-6份。
优选的,所述的组份包括:膨胀珍珠岩  20份,甲基硅酸钠 2份, 水玻璃 4份。
所述的膨胀珍珠岩的色度相同,粒径的大小为R,其中3.01≤R≤4mm。
所述的轻质防火保温板的加工方法,包括以下步骤:
(1)称取上述重量份的膨胀珍珠岩、甲基硅酸钠和水玻璃;
(2)将甲基硅酸钠和水玻璃充分混合搅拌;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内,所述的挤压的压强为50-100Mpa;
(5)脱模后进行干燥,干燥温度为50-300℃,干燥时间为4-24小时;
(6)即得保温板。
本发明的优点是:通过对膨胀珍珠岩的粒径进行筛选,然后为原材料进行加工,大大降低了保温板的重量,提高了保温效果,防潮效果明显,通过甲基硅酸钠和水玻璃的充分混合后,大大提高了珍珠岩颗粒之间的粘合力;同时由于加固框的作用,提高了保温板韧度,不易发生脆裂,使得抗拉强度大大提高。
具体实施方式
实施例1:(以下单位为重量份)
(1)称取膨胀珍珠岩10份、甲基硅酸钠1份和水玻璃2份;其中珍珠岩粒径的大小为R,其中3.01 mm≤R≤4mm,当珍珠岩的粒径小于3或者大于4mm的时候,加工而成的保温板容易脆断,和甲基硅酸钠、水玻璃混合的时候不能得到最佳的混合效果;因此当珍珠岩粒径太大或者太小的时候,对甲基硅酸钠和水玻璃要求的份数,以及混合以后均不能满足实际的需求,通过这一比例,减少了水玻璃和甲基硅酸钠的用量,节约了原材料;
(2)将甲基硅酸钠和水玻璃充分混合搅拌,通过这一步骤,大大缩短了下一步膨胀珍珠岩与甲基硅酸钠和水玻璃的混合时间;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内,挤压的压强为50Mpa;
(5)脱模后进行干燥, 干燥温度为50℃,干燥时间为4小时;
(6)即得保温板。
实施例2:(以下单位为重量份):
(1)称取膨胀珍珠岩20份、甲基硅酸钠2份和水玻璃4份;
(2)将甲基硅酸钠和水玻璃充分混合搅拌;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内,挤压的压强为70Mpa;
(5)脱模后进行干燥, 干燥温度为100℃,干燥时间为10小时;
(6)即得保温板。
实施例3:(以下单位为重量份):
(1)称取膨胀珍珠岩30份、甲基硅酸钠3份和水玻璃6份;
(2)将甲基硅酸钠和水玻璃充分混合搅拌;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内,挤压的压强为90Mpa;
(5)脱模后进行干燥, 干燥温度为200℃,干燥时间为16小时;
(6)即得保温板。
实施例4:(以下单位为重量份):
(1)称取膨胀珍珠岩30份、甲基硅酸钠3份和水玻璃6份;
(2)将甲基硅酸钠和水玻璃充分混合搅拌;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内,挤压的压强为100Mpa;
(5)脱模后进行干燥, 干燥温度为300℃,干燥时间为24小时;
(6)即得保温板。

Claims (6)

1.一种轻质防火保温板,其特征在于,包括以下重量份的各组份组成:膨胀珍珠岩  10-30份,甲基硅酸钠 1-3份, 水玻璃 2-6份。
2.根据权利要求1所述的轻质防火保温板,其特征在于,所述的组份包括:膨胀珍珠岩  20份,甲基硅酸钠 2份, 水玻璃 4份。
3.根据权利要求1或2所述的轻质防火保温板的加工方法,其特征在于,所述的膨胀珍珠岩的色度相同,粒径的大小为R,其中3.01≤R≤4mm。
4.根据权利要求3所述的轻质防火保温板的加工方法,其特征在于,包括以下步骤:
(1)称取上述重量份的膨胀珍珠岩、甲基硅酸钠和水玻璃;
(2)将甲基硅酸钠和水玻璃充分混合搅拌;
(3)将混合后的甲基硅酸钠与水玻璃在滚筒中与膨胀珍珠岩充分混合,得到混合物料;
(4)将混合物料置入模具框中进行挤压,其中,首先将物料总份数的1/3置入模具底层,均匀摊铺,然后放入一层加固框,然后将剩余的2/3物料均匀摊铺在模具框内;
(5)脱模后进行干燥;
(6)即得保温板。
5.根据权利要求3所述的轻质防火保温板的加工方法,其特征在于,所述的步骤(4)中的压强为50-100Mpa。
6.根据权利要求3所述的轻质防火保温板的加工方法,其特征在于,所述的步骤(5)中的干燥温度为50-300℃,干燥时间为4-24小时。
CN 201110208240 2011-07-05 2011-07-25 轻质防火保温板的加工方法 Expired - Fee Related CN102320807B (zh)