CN101955214A - 一种赤泥制备的聚合硫酸硅铝混凝剂 - Google Patents
一种赤泥制备的聚合硫酸硅铝混凝剂 Download PDFInfo
- Publication number
- CN101955214A CN101955214A CN 201010297485 CN201010297485A CN101955214A CN 101955214 A CN101955214 A CN 101955214A CN 201010297485 CN201010297485 CN 201010297485 CN 201010297485 A CN201010297485 A CN 201010297485A CN 101955214 A CN101955214 A CN 101955214A
- Authority
- CN
- China
- Prior art keywords
- red mud
- coagulant
- filtrate
- polysulphate
- silicon aluminum
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
本发明属于环境保护技术领域,涉及一种环保的高分子聚合混凝剂。该聚合硫酸硅铝混凝剂原料按质量百分比为:氢氧化钾处理后的滤液35-40%、硫酸处理后的滤液45-55%、稳定剂10-15%。该聚合硫酸硅铝混凝剂的研制不仅可以充分提取赤泥中的活性成分,而且应用于处理工业含镉废水,也为当前废水处理领域提供了新型水处理药剂。聚合硫酸硅铝混凝剂以赤泥为主要原料,不仅产品性能优良,稳定性好,而且由于采用赤泥为载体使制备的混凝剂对于工业含镉废水中的多种有害物质均能产生良好的去除效果。赤泥制备混凝剂不仅解决了环境污染问题,而且也为水处理领域提供了有利的技术支持。
Description
技术领域
本发明专利属于环保技术领域,具体涉及到利用赤泥为原料制备聚合硫酸硅铝混凝剂。
背景技术
赤泥是氧化铝工业排放的红色粉泥状废料,属强碱性有害残渣。目前,赤泥的处置要占用大量的土地,耗费较多的堆场和维护费用以及污染周围的环境,同时赤泥中的可利用成分不能得到合理的利用,造成了资源的浪费。因此,赤泥的资源化利用是国内外环保领域的一个研究热点。
赤泥的化学成分和矿物组成主要取决于铝土矿的成分、生产氧化铝的方法和生产过程中添加剂的物质成分等。一般说来,SiO2,Al2O3是赤泥中主要存在的氧化物,同时也是合成复合型混凝剂的有效成分。因此,赤泥制备无机高分子混凝剂可充分利用赤泥的活性成分,最大限度地发挥赤泥成分优势,用于处理工业废水,达到以废治废的目的,提高赤泥资源综合利用水平。
发明内容
为解决赤泥的综合利用问题,本发明提供了一种以赤泥为原料制备的聚合硫酸硅铝混凝剂。
本发明利用赤泥制备聚合硫酸硅铝混凝剂。将烘干后的赤泥首先在氢氧化钾溶液中浸泡,水浴加热一定时间,获得滤液,调节滤液pH值;再将滤渣用硫酸溶液浸取后过滤,取滤液备用。在一定温度下,将氢氧化钾滤液与硫酸滤液按一定比例混合搅拌,同时加入稳定剂,陈化后即制得聚合硫酸硅铝混凝剂。聚合硫酸硅铝混凝剂按各成分质量百分比为氢氧化钾处理后的滤液35-40%、硫酸处理后的滤液45-55%、稳定剂10-15%。
利用赤泥制备聚合硫酸硅铝混凝剂,不仅可以充分提取赤泥中的活性成分,而且应用于处理工业含镉废水,也为当前废水处理领域提供了新型水处理药剂。聚合硫酸硅铝混凝剂以赤泥为主要原料,不仅产品性能优良,稳定性好,而且由于采用赤泥为载体使制备的混凝剂对于工业含镉废水中的多种有害物质均能产生良好的去除效果。赤泥制备混凝剂不仅解决了环境污染问题,而且也为水处理领域提供了有利的技术支持。
具体实施方式
实施例一:
取经烘干后的赤泥,在2.0mol/L的氢氧化钾溶液中浸泡,55℃水浴下加热15h,冷却后提取滤液,调节滤液pH至1.2;再将剩余残渣浸泡在20%硫酸溶液中一定时间后取滤液。在40℃下,将氢氧化钾处理后的滤液与硫酸处理后的滤液按比例混合、搅拌,加入一定量的稳定剂,熟化4d即得到聚合硫酸硅铝混凝剂。本发明的聚合硫酸硅铝混凝剂,是由以下质量百分比的原料制成:
氢氧化钾滤液 35%
硫酸滤液 55%
氯化镁 10%
氢氧化钾、硫酸、氯化镁均为工业级,聚合硫酸硅铝混凝剂为工业级液体。
实施例二:
取经烘干后的赤泥,在2.2mol/L的氢氧化钾溶液中浸泡,60℃水浴下加热13h,冷却后提取滤液,调节滤液pH至1.3;再将剩余残渣浸泡在25%硫酸溶液中一定时间后取滤液。在45℃下,将氢氧化钾处理后的滤液与硫酸处理后的滤液按比例混合、搅拌,加入一定量的稳定剂,熟化5d即得到聚合硫酸硅铝混凝剂。本发明的聚合硫酸硅铝混凝剂,是由以下质量百分比的原料制成:
氢氧化钾滤液 38%
硫酸滤液 50%
碳酸镁 12%
氢氧化钾、硫酸、碳酸镁均为工业级,聚合硫酸硅铝混凝剂为工业级液体。
实施例三:
取经烘干后的赤泥,在2.5mol/L的氢氧化钾溶液中浸泡,65℃水浴下加热10h,冷却后提取滤液,调节滤液pH至1.4;再将剩余残渣浸泡在30%硫酸溶液中一定时间后取滤液。在50℃下,将氢氧化钾处理后的滤液与硫酸处理后的滤液按比例混合、搅拌,加入一定量的稳定剂,熟化6d即得到聚合硫酸硅铝混凝剂。本发明的聚合硫酸硅铝混凝剂,是由以下质量百分比的原料制成:
氢氧化钾滤液 40%
硫酸滤液 45%
碳酸氢镁 15%
氢氧化钾、硫酸、碳酸氢镁均为工业级,聚合硫酸硅铝混凝剂为工业级液体。
Claims (2)
1.一种以赤泥为原料制备的聚合硫酸硅铝混凝剂,其特征在于:按质量百分比氢氧化钾处理后的滤液35-40%、硫酸处理后的滤液45-55%、稳定剂10-15%。
2.根据权利1所述的以赤泥为原料制备的聚合硫酸硅铝混凝剂,其特征在于:稳定剂是氯化镁、碳酸镁、碳酸氢镁中的一种。