CN101935954B - Fabric pattern dyeing method and dyeing instrument thereof - Google Patents

Fabric pattern dyeing method and dyeing instrument thereof Download PDF

Info

Publication number
CN101935954B
CN101935954B CN2010102661937A CN201010266193A CN101935954B CN 101935954 B CN101935954 B CN 101935954B CN 2010102661937 A CN2010102661937 A CN 2010102661937A CN 201010266193 A CN201010266193 A CN 201010266193A CN 101935954 B CN101935954 B CN 101935954B
Authority
CN
China
Prior art keywords
dyeing
wrinkle
fabric
utensil
netted
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN2010102661937A
Other languages
Chinese (zh)
Other versions
CN101935954A (en
Inventor
梁佳钧
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHEJIANG QIAOTINGTING GARMENTS CO Ltd
Original Assignee
ZHEJIANG QIAOTINGTING GARMENTS CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHEJIANG QIAOTINGTING GARMENTS CO Ltd filed Critical ZHEJIANG QIAOTINGTING GARMENTS CO Ltd
Priority to CN2010102661937A priority Critical patent/CN101935954B/en
Publication of CN101935954A publication Critical patent/CN101935954A/en
Application granted granted Critical
Publication of CN101935954B publication Critical patent/CN101935954B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a fabric pattern dyeing method and a dyeing instrument thereof and belongs to the technical field of fabric dyeing technology. The method comprises the following steps of: (1), placing a fabric on a worktable and creasing the fabric until all edges and corners of the fabric are creased together to form a creasing body; (2), placing the creasing body in the dyeing instrument and closing an opening of the dyeing instrument, wherein the size and the shape of the dyeing instrument are matched with the size and the shape of the creasing body; and (3), selecting a dye and an auxiliary agent of the dyed colour and setting a dyeing process according to the raw material of the dyed fabric. Patterns dyed by the invention are natural and irregular; the dyeing process is simple; the dyeing time is short; and the efficiency is high.

Description

A kind of fabric fleuron colouring method and dyeing utensil thereof
Technical field
The present invention relates to a kind of colouring method and dyeing utensil thereof of fabric fleuron, belong to the fabric dyeing process technical field.
Background technology
The colored shape of existing textile fabric is knitted through look or the stamp mode realizes; Fabric after the dyeing generally all is a plain color; Embodying colored shape through dyeing also has several kinds of modes at present, and the one, dye colored shape with different dyes after being woven into colored shape with different material, this flower shape is that certain rule is arranged; The 2nd, tie dyeing is dyed colored shape afterwards through fabric is tied up, and flower shape has certain vestige of tying up after the tie dyeing, and flower shape is not too natural, and it is more that the time is tied up in cost.
Summary of the invention
The purpose of this invention is to provide colouring method and the dyeing utensil thereof of fabric through being nature flower shape after dyeing.
To achieve these goals, the technical scheme that the present invention adopted is:
A kind of fabric fleuron colouring method comprises the steps:
(1) fabric be placed on grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body.To not wrinkle that body is loose to be opened this moment, remain the last corrugation attitude of grabbing.Colored shape after dying is if desired grabbed spaced point when wrinkling more so; Colored shape after dying if desired is littler, point off density when grabbing wrinkle so.
(2) put into the dyeing utensil with above-mentioned without the loose wrinkle body of opening, and the opening of the utensil that will dye closes, the size of this dyeing utensil, shape and wrinkle body are complementary, to be used for fixing the shape of the body that wrinkles.The corresponding fabric (a wrinkle body) of placing of dyeing utensil.During dyeing,, can simultaneously a plurality of coloration of textile materials utensils that are equipped be placed in the big sack together, wait to dye for enhancing productivity.
(3) according to the raw material of institute's dyeing and weaving thing, select institute to dye the dyestuff and the auxiliary agent of color, the formulation dyeing is following:
1. cotton, regenerated celulose fibre or silk like coloration of textile materials technology and flow process
The same REACTIVE DYES of dyeing utensil, glauber salt, soda ash that the wrinkle body is housed put into together be warmed up to 60 ℃ → insulation 20-40 minute → draining → hot water wash → 90 in the dye vat and ℃ soap → wash → take out the utensil that dyes, the wrinkle body of the inside is taken out after washing → softness;
2. polyamide fibre, acrylic fiber coloration of textile materials technology and flow process
Add dyestuff and auxiliary agent directly be warmed up to 80 ℃ → dropping into the dyeing utensil that the wrinkle body is housed continues to be warmed up to 100 ℃ → insulation draining → hot water wash → washing → 70 ℃ of-80 ℃ of fixation of polyamide fibre dark colour after 5-10 minute; Acrylic fibers dark 60 ℃-80 ℃ soap → wash → take out the utensil that dyes, the wrinkle body of the inside is taken out after washing → softness;
3. the dyeing of terylene kind fabric and flow process
Add dyestuff and auxiliary agent directly be warmed up to 80 ℃ → dropping into the dyeing utensil that the wrinkle body is housed continues to be warmed up to behind 125 ℃ → insulation 5-10 minute → cool to 80 ℃ draining → hot water wash → washing → 80 ℃ reduction cleaning → washing → taking-up utensil that dyes, and the wrinkle body of the inside is taken out after washing → softness.
The dyeing utensil that is used in a kind of fabric fleuron colouring method comprises following making step:
(1) selecting for use of material: DYED FABRICS is cotton, regenerated celulose fibre, polyamide fibre, then selects for use the netted lining of terylene to make; DYED FABRICS is a terylene, then selects for use the netted lining of netted cotton or polypropylene fibre to make;
(2) preparation method: according to desired shape and size; Make model; According to the netted lining of model cutting terylene or netted cotton fabric or the netted lining of polypropylene fibre, two linings that cut are sewed up sack that has opening of formation, this opening supplies DYED FABRICS turnover to use.After DYED FABRICS puts in, opening is tied up.It is tight that opening is tied up, and the colored shape after dying so more obviously; The pine that opening is tied up, the colored shape after dying so is fuzzy.
Described dyeing utensil is any one in rectangle, ellipse, doleiform, the Pear-Shaped.
The present invention has following outstanding advantage and good effect:
1. do not knit, as long as just can dye colored shape through dyeing through stamp and look.
Institute's dyeing flower shape nature, do not have rule, can dye with colour system flower shape through once pack dyeing, also can dye double-coloredly or polychrome flower shape through secondary or repeatedly pack dyeing.
3. the shape of spending shape and size need not complicated design design as long as control through the degree of tightness of grabbing wrinkle mode and pack, and be simple to operate, control easily, and easily-learned easily mastered, device therefor or device are simple, and the dyeing cost is low, and bigger profit margin is arranged.
4. dyeing is simple, and dying operation is simple, only needs directly to feed in raw material, just directly heat up can, need not temperature control, need not to pay close attention to dyeing generation look flower.
5. dyeing time is short, and the heating-up time is fast, temperature retention time is short, just can dye a cylinder in general one hour, and efficient is high, and the output value is high, and variety renovation is fast, suitable many kinds, small lot batch manufacture.
The specific embodiment
Through specific embodiment the present invention is described further below, but the present invention is not limited by following examples.
Embodiment 1:
Textile is formed: 60 cotton 75%, 20/30 cladded yarns 25%
Product: camisole and panties, about 50 grams of camisole, about 35 grams of panties
Color: claret
Operating instruction: the rectangle sack rigging band vest of making 15cmx30cm; 10cmx20cm rectangle sack dress panties; Be placed on single-piece the said goods and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription and technology:
A oxygen floats the oil removing prescription:
Degreaser FT-128 1g/L
Scouring agent L-100Z 0.5g/L
Hydrogen peroxide solution 2.5g/L
Oxygen floats auxiliary agent 1.5g/L
The B dyeing prescription:
The vapour Bark swells the red S-B 2.5% of sauce
The vapour Bark swells yellow FN-R 0.5%
The vapour Bark swells blue FN-R 0.35%
Glauber salt 50g/L
Soda ash 20g/L
The technological operation step:
Adding hydrogen peroxide solution, oxygen floats 95 ℃ of oxygen of auxiliary agent and fabric → directly be warmed up to and floats the fabric that cools to behind the 30min after 60 ℃ of draining → hot water wash → washing → dehydration → oven dry → oxygen is floated and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the sack that ties an opening solid shape → fabric only is housed to 4-5 separately in the wrinkle body → sack of choosing of packing into together put in the big bag wait to dye → the same REACTIVE DYES of big bag, glauber salt, soda ash put into dye vat together be warmed up to 60 ℃ → insulation, 30 minutes → draining → hot water wash → 90 and ℃ soap → wash → take out sack, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 2:
Textile is formed: 60 cotton 75%, 20/30 cladded yarns 25%
Product: camisole and panties, about 50 grams of camisole, about 35 grams of panties
Color: claret
Operating instruction: the rectangle sack rigging band vest of making 15cmx30cm; 10cmx20cm rectangle sack dress panties; Be placed on single-piece the said goods and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription and technology:
A oxygen floats the oil removing prescription:
Degreaser FT-128 1g/L
Scouring agent L-100Z 0.5g/L
Hydrogen peroxide solution 2.5g/L
Oxygen floats auxiliary agent 1.5g/L
The B dyeing prescription:
The vapour Bark swells the red S-B 2.5% of sauce
The vapour Bark swells yellow FN-R 0.5%
The vapour Bark swells blue FN-R 0.35%
Glauber salt 50g/L
Soda ash 20g/L
The technological operation step:
Adding hydrogen peroxide solution, oxygen floats 95 ℃ of oxygen of auxiliary agent and fabric → directly be warmed up to and floats the fabric that cools to behind the 30min after 60 ℃ of draining → hot water wash → washing → dehydration → oven dry → oxygen is floated and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the sack that ties an opening solid shape → fabric only is housed to 4-5 separately in the wrinkle body → sack of choosing of packing into and together put in the big bag and wait to dye → the same REACTIVE DYES of big bag, glauber salt, soda ash are put into dye vat together be warmed up to 20 minutes → draining → hot water wash of 60 ℃ → insulation → soap → wash → take out sack, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 3:
Textile is formed: 60 cotton 75%, 20/30 cladded yarns 25%
Product: camisole and panties, about 50 grams of camisole, about 35 grams of panties
Color: claret
Operating instruction: the rectangle sack rigging band vest of making 15cmx30cm; 10cmx20cm rectangle sack dress panties; Be placed on single-piece the said goods and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription and technology:
A oxygen floats the oil removing prescription:
Degreaser FT-128 1g/L
Scouring agent L-100Z 0.5g/L
Hydrogen peroxide solution 2.5g/L
Oxygen floats auxiliary agent 1.5g/L
The B dyeing prescription:
The vapour Bark swells the red S-B 2.5% of sauce
The vapour Bark swells yellow FN-R 0.5%
The vapour Bark swells blue FN-R 0.35%
Glauber salt 50g/L
Soda ash 20g/L
The technological operation step:
Adding hydrogen peroxide solution, oxygen floats 95 ℃ of oxygen of auxiliary agent and fabric → directly be warmed up to and floats the fabric that cools to behind the 30min after 60 ℃ of draining → hot water wash → washing → dehydration → oven dry → oxygen is floated and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the sack that ties an opening solid shape → fabric only is housed to 4-5 separately in the wrinkle body → sack of choosing of packing into together put in the big bag wait to dye → the same REACTIVE DYES of big bag, glauber salt, soda ash put into dye vat together be warmed up to 60 ℃ → insulation, 40 minutes → draining → hot water wash → 90 and ℃ soap → wash → take out sack, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 4:
Textile is formed: 65% 70D/68F polyamide fibre, 22.3% 20/30-12F cladded yarn, 10.2% end crotch cotton yarn, the waist elastic of 2.5%140D.
Product: triangle pants and boxers, every heavily about 30 grams of trousers
Color: navy blue
Operating instruction: make 10cmx20cm rectangle sack; Be placed on single-piece panties or swimming trunk and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the wrinkle body, put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription:
Lanaset 2R blue 0.58%
The red B 0.09% of Lanaset sauce
Glacial acetic acid 1g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 100 ℃ → be incubated 10 minutes after draining → hot water wash → washing → 70 ℃ of fixation → washings of polyamide fibre dark colour → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 5:
Textile is formed: 65% 70D/68F polyamide fibre, 22.3% 20/30-12F cladded yarn, 10.2% end crotch cotton yarn, the waist elastic of 2.5%140D.
Product: triangle pants and boxers, every heavily about 30 grams of trousers
Color: navy blue
Operating instruction: make 10cmx20cm rectangle sack; Be placed on single-piece panties or swimming trunk and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the wrinkle body, put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription:
Lanaset 2R blue 0.58%
The red B 0.09% of Lanaset sauce
Glacial acetic acid 1g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 100 ℃ → be incubated 5 minutes after draining → hot water wash → washing → 80 ℃ of fixation → washings of polyamide fibre dark colour → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 6:
Textile is formed: 65% 70D/68F polyamide fibre, 22.3% 20/30-12F cladded yarn, 10.2% end crotch cotton yarn, the waist elastic of 2.5%140D.
Product: triangle pants and boxers, every heavily about 30 grams of trousers
Color: navy blue
Operating instruction: make 10cmx20cm rectangle sack; Be placed on single-piece panties or swimming trunk and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form the wrinkle body, put in the sack that size, shape are complementary with it, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of terylene to process.
Dyeing prescription:
Lanaset 2R blue 0.58%
The red B 0.09% of Lanaset sauce
Glacial acetic acid 1g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 100 ℃ → be incubated 8 minutes after draining → hot water wash → washing → 75 ℃ of fixation → washings of polyamide fibre dark colour → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 7
Textile is formed: 68% 70D/75F COOLMAX terylene, 29.5% 20/30-12F cladded yarn, the waist elastic of 2.5%140D.
Product: the four fens trousers that move, every heavily about 60 grams of trousers
Color: black
Operating instruction: make 15cmx30cm rectangle sack; Be placed on four fens trousers of single-piece motion and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the above-mentioned sack, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of polypropylene fibre to process.
Dyeing prescription:
Disperse black ECO 5%
Glacial acetic acid 1.5g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 125 ℃ → cool to 80 ℃ after being incubated 5 minutes after draining → hot water wash → washing → 80 ℃ reduction cleaning → washing → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 8
Textile is formed: 68% 70D/75F COOLMAX terylene, 29.5% 20/30-12F cladded yarn, the waist elastic of 2.5%140D.
Product: the four fens trousers that move, every heavily about 60 grams of trousers
Color: black
Operating instruction: make 15cmx30cm rectangle sack; Be placed on four fens trousers of single-piece motion and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the above-mentioned sack, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use netted cotton fabric to process.
Dyeing prescription:
Disperse black ECO 5%
Glacial acetic acid 1.5g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 125 ℃ → cool to 80 ℃ after being incubated 10 minutes after draining → hot water wash → washing → 80 ℃ reduction cleaning → washing → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.
Embodiment 9
Textile is formed: 68% 70D/75F COOLMAX terylene, 29.5% 20/30-12F cladded yarn, the waist elastic of 2.5%140D.
Product: the four fens trousers that move, every heavily about 60 grams of trousers
Color: black
Operating instruction: make 15cmx30cm rectangle sack; Be placed on four fens trousers of single-piece motion and grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body; Put in the above-mentioned sack, the opening of tightening sack is with the shape of fixed product and wait to dye.Sack selects for use the netted lining of polypropylene fibre to process.
Dyeing prescription:
Disperse black ECO 5%
Glacial acetic acid 1.5g/L
The technological operation step:
Adding 80 ℃ in degreaser, refining agent and fabric → directly be warmed up to handles and cools to 60 ℃ of draining → washings → dehydration → oven dry → the fabric after the refining behind the 30min and be placed on and grab wrinkle on the work top; All wrinkle together until the fabric corner; Form tie in the wrinkle body → sack of choosing of packing into the opening solid shape → 4-5 sack put into wait in the big bag to dye → add dyestuff and glacial acetic acid directly be rapidly heated 80 ℃ → add big bag to be dyed directly be rapidly heated 125 ℃ → cool to 80 ℃ after being incubated 8 minutes after draining → hot water wash → washing → 80 ℃ reduction cleaning → washing → taking-up big bag, the wrinkle body of the inside is taken out after washing → softness.

Claims (3)

1. a fabric fleuron colouring method is characterized in that comprising the steps:
(1) fabric be placed on grab wrinkle on the work top, until the fabric corner all wrinkle hold together together, form the wrinkle body;
(2) body that will wrinkle is put into the dyeing utensil, and the opening of the utensil that will dye closes, and the size of this dyeing utensil, shape and wrinkle body are complementary;
(3) according to the raw material of institute's dyeing and weaving thing, select institute to dye the dyestuff and the auxiliary agent of color, the formulation dyeing is following:
1. cotton, regenerated celulose fibre or silk like coloration of textile materials technology and flow process
The same REACTIVE DYES of dyeing utensil, glauber salt, soda ash that the wrinkle body is housed put into together be warmed up to 60 ℃ → insulation 20-40 minute → draining → hot water wash → 90 in the dye vat and ℃ soap → wash → take out the utensil that dyes, the wrinkle body of the inside is taken out after washing → softness;
2. polyamide fibre, acrylic fiber coloration of textile materials technology and flow process
Add dyestuff and auxiliary agent directly be warmed up to 80 ℃ → dropping into the dyeing utensil that the wrinkle body is housed continues to be warmed up to 100 ℃ → insulation draining → hot water wash → washing → 70 ℃ of-80 ℃ of fixation of polyamide fibre dark colour after 5-10 minute; Acrylic fibers dark 60 ℃-80 ℃ soap → wash → take out the utensil that dyes, the wrinkle body of the inside is taken out after washing → softness;
3. the dyeing of terylene kind fabric and flow process
Add dyestuff and auxiliary agent directly be warmed up to 80 ℃ → dropping into the dyeing utensil that the wrinkle body is housed continues to be warmed up to behind 125 ℃ → insulation 5-10 minute → cool to 80 ℃ draining → hot water wash → washing → 80 ℃ reduction cleaning → washing → taking-up utensil that dyes, and the wrinkle body of the inside is taken out after washing → softness;
Said dyeing utensil comprises following making step:
(1) selecting for use of material: DYED FABRICS is cotton, regenerated celulose fibre, polyamide fibre, then selects for use the netted lining of terylene to make; DYED FABRICS is a terylene, then selects for use the netted lining of netted cotton or polypropylene fibre to make;
(2) preparation method: according to desired shape and size, make model,, two linings that cut are sewed up sack that has opening of formation according to the netted lining of model cutting terylene or netted cotton fabric or the netted lining of polypropylene fibre.
2. the dyeing utensil that is used in the fabric fleuron colouring method as claimed in claim 1 is characterized in that comprising following making step:
(1) selecting for use of material: DYED FABRICS is cotton, regenerated celulose fibre, polyamide fibre, then selects for use the netted lining of terylene to make; DYED FABRICS is a terylene, then selects for use the netted lining of netted cotton or polypropylene fibre to make;
(2) preparation method: according to desired shape and size, make model,, two linings that cut are sewed up sack that has opening of formation according to the netted lining of model cutting terylene or netted cotton fabric or the netted lining of polypropylene fibre.
3. dyeing utensil as claimed in claim 2 is characterized in that: described dyeing utensil is any one in rectangle, ellipse, the Pear-Shaped.
CN2010102661937A 2010-08-25 2010-08-25 Fabric pattern dyeing method and dyeing instrument thereof Active CN101935954B (en)